Nitrogen / sulfur modified activated carbon loaded monatomic noble metal catalyst, preparation method and application

The activated carbon-supported single-atom precious metal catalysts with nitrogen/sulfur modified are solved, and the problems of easy corrosion and high cost of traditional catalysts are improved, catalytic activity and stability are achieved, and the methanol carbonylation reaction is efficient, which is suitable for industrial production.

CN118904356APending Publication Date: 2024-11-08DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310505725.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-06
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The homogeneous catalysts such as Rh or Ir used in traditional methanol carbonylation reactions have problems such as easy equipment corrosion, catalyst recovery and high product separation costs, catalyst poisoning, carbon deposits and metal sintering. The heterogeneous catalysts have the reaction activity, stability and There are still shortcomings in metal loss.

Method used

Develop a nitrogen/sulfur modified activated carbon supported single-atom noble metal catalyst, which regulates the microstructure of the activated carbon support surface through heteroatom modification, anchors the metal through chemical bonds, improves catalytic activity and stability, and uses nitrogen/sulfur precursors to react with activated carbon Later, it coordinates with the precious metal precursor to form a stable single-atom precious metal catalyst.

Benefits of technology

The stable loading and efficient catalysis of the catalyst are achieved, the reaction pressure is reduced, the catalytic activity and stability is improved, the operation is simple, the conditions are mild, and the applicability is strong. It replaces the complex polymer support and improves the efficiency of methanol carbonylation reaction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904356A_ABST
    Figure CN118904356A_ABST
Patent Text Reader

Abstract

The invention discloses a nitrogen / sulfur modified activated carbon loaded monatomic noble metal catalyst, a preparation method and application, the preparation method comprises the following steps: (1) performing reaction I, drying I and roasting I on a mixture I containing activated carbon and a nitrogen / sulfur precursor solution to obtain nitrogen / sulfur modified activated carbon; (2) reacting the nitrogen / sulfur modified activated carbon with iodomethane II in an inactive atmosphere to obtain iodomethane modified activated carbon; and (3) carrying out a reaction III on the mixture II containing the methyl iodide modified activated carbon and the noble metal precursor solution, and drying the III to obtain the nitrogen / sulfur modified activated carbon loaded monatomic noble metal catalyst. The modified activated carbon carrier stably loaded monatomic noble metal catalyst and the preparation method thereof are simple to operate, mild in condition and high in universality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a nitrogen / sulfur-modified activated carbon-supported single-atom precious metal catalyst, a preparation method and an application thereof, and belongs to the field of new catalyst technology materials. Background Art

[0002] As an important bulk organic chemical product, acetic acid is widely used in industries such as plastics, chemicals and medicine. Its global annual production exceeds 20 million tons, and Asia accounts for more than two-thirds of global consumption. The main industrial acetic acid production processes include acetaldehyde oxidation, ethylene direct oxidation, light hydrocarbon liquid phase oxidation and methanol carbonylation. Among them, methanol carbonylation is one of the main methods for producing acetic acid in the world, as it not only has cheap and readily available raw materials, but also has high selectivity for the product acetic acid and few by-products. The Cativa, Celanese and UOP / Chiyoda processes developed successively. Acetica and other processes have made different improvements in the device capacity, catalyst development and reaction process involved in the process. In addition to some of the low-pressure carbonylation processes developed independently, most of my country still relies on foreign technology, and the production process, especially the catalyst performance and cost control, is still somewhat behind that of foreign countries. Therefore, the development of new acetic acid production processes with independent intellectual property rights in my country has far-reaching economic and strategic significance for improving my country's acetic acid production capacity and expanding domestic and foreign markets.

[0003] Homogeneous catalyst systems such as Rh or Ir used in traditional methanol carbonylation reactions have problems such as easy equipment corrosion, high catalyst recovery and product separation costs. Heterogeneous catalysts have obvious advantages in recovery and reaction energy consumption, and are one of the effective ways to solve the above problems. However, catalyst poisoning, carbon deposition and metal sintering are still the main problems; the oxidation, reduction, chlorination, oxychlorination and halogenated hydrocarbon heat treatment methods developed from them have been proven to reduce the metal particle size and improve the dispersion to a certain extent, but the operating conditions are harsh, the universality is low, and the dispersion of precious metals still has room for improvement. At present, related research is mainly focused on the development of supported catalysts, and the carriers mainly include SiO2, Al2O3, activated carbon, ionic liquids and porous polymers. Compared with homogeneous catalysts, heterogeneous catalysts have obvious advantages in catalyst recovery and reaction energy consumption, but they are still insufficient in reaction activity, stability, metal loss, etc. At the same time, catalyst poisoning, carbon deposition and metal sintering are still the main problems. Summary of the invention

[0004] The technical problem to be solved by the present application is to provide a nitrogen / sulfur-modified activated carbon carrier loaded with a single-atom precious metal catalyst and a preparation method thereof in view of the deficiencies of the above-mentioned prior art. The catalyst regulates the surface microstructure of the activated carbon carrier through heteroatom modification, imparts functional sites to the activated carbon, anchors the metal through chemical bonds, effectively stabilizes the metal single atom, and improves the catalytic activity and stability.

[0005] To achieve the improvement of catalytic activity and stability, it is necessary to reduce the size of supported catalyst metal particles while stabilizing the anchoring of metal active centers.

[0006] According to one aspect of the present application, a nitrogen / sulfur modified activated carbon-supported single-atom noble metal catalyst is provided, wherein the activated carbon-supported single-atom noble metal catalyst comprises a noble metal, a non-metal, and a carrier;

[0007] The noble metal and the non-metal are fixedly supported on the carrier;

[0008] The noble metal is selected from at least one of Rh, Ru, Pd, Ir, Mo, Pt and Ag;

[0009] The non-metal is nitrogen and / or sulfur;

[0010] The carrier is activated carbon.

[0011] Optionally, the mass of the noble metal is 0.2 to 5.0 wt.% of the mass of the activated carbon-supported single-atom noble metal catalyst.

[0012] According to another aspect of the present application, a method for preparing the above-mentioned nitrogen / sulfur-modified activated carbon-supported single-atom noble metal catalyst is provided, and the preparation method comprises the following steps:

[0013] (1) reacting a mixture I containing activated carbon and a nitrogen / sulfur precursor solution, drying I, and calcining I to obtain nitrogen / sulfur modified activated carbon;

[0014] (2) reacting the nitrogen / sulfur modified activated carbon with methyl iodide under an inert atmosphere to obtain methyl iodide modified activated carbon;

[0015] (3) reacting a mixture II containing iodomethane-modified activated carbon and a noble metal precursor solution, and drying III to obtain a nitrogen / sulfur-modified activated carbon-supported single-atom noble metal catalyst.

[0016] Optionally, the nitrogen / sulfur precursor solution is selected from at least one of a nitrogen precursor solution, a sulfur precursor solution, and a nitrogen-sulfur precursor solution.

[0017] Optionally, the nitrogen precursor solution is melamine.

[0018] Optionally, the sulfur precursor solution is selected from 2,2-bithiophene and / or 2-benzyl disulfide.

[0019] Optionally, the nitrogen-sulfur precursor solution is selected from thiourea and / or thioacetamide.

[0020] Optionally, the mass ratio of the nitrogen precursor solution to the activated carbon is 1:1 to 10:1.

[0021] Optionally, the mass ratio of the nitrogen precursor solution to the activated carbon is selected from any value of 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1 or a range between any two of the above points.

[0022] Optionally, the mass ratio of the sulfur precursor to the activated carbon is 0.2:1 to 10:1.

[0023] Optionally, the mass ratio of the sulfur precursor to the activated carbon is selected from any value of 0.2:1, 0.5:1, 1:1, 2:1, 4:1, 6:1, 8:1, 10:1 or a range between any two of the above points.

[0024] Optionally, the mass ratio of the nitrogen-sulfur precursor to the activated carbon is 0.2:1 to 5:1.

[0025] Optionally, the mass ratio of the nitrogen-sulfur precursor to the activated carbon is selected from any value of 0.2:1, 0.5:1, 1:1, 2:1, 3:1, 5:1 or a range between any two of the above points.

[0026] Optionally, the noble metal precursor solution is selected from at least one of carbonyl rhodium chloride dimer, hexacarbonyl ruthenium chloride, dicarbonyl iridium acetylacetonate, chloroplatinic acid, palladium chloride, molybdenum acetylacetonate, and silver nitrate.

[0027] Optionally, the mass ratio of the nitrogen / sulfur modified activated carbon to methyl iodide is 1:10 to 1:50.

[0028] Optionally, the mass ratio of the iodomethane-modified activated carbon to the noble metal precursor solution is 1:5 to 1:20.

[0029] Optionally, in step (1), the temperature of reaction I is 150-180° C., and the time of reaction I is 5-12 h.

[0030] Optionally, the temperature of the reaction I is selected from any value of 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, or a range between any two of the above points.

[0031] Optionally, the reaction time I is selected from any value among 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, or a range between any two of the above points.

[0032] Optionally, the temperature of the drying I is 80 to 150° C., and the time of the drying I is 12 to 24 hours.

[0033] Optionally, the drying temperature I is selected from any value of 80°C, 90°C, 100°C, 120°C, 150°C or a range between any two of the above points.

[0034] Optionally, the drying time I is selected from any value among 12h, 14h, 16h, 18h, 20h, 22h, 24h or a range value between any two of the above points.

[0035] Optionally, the temperature of the calcination I is 400-900° C., and the time of the calcination I is 2-12 hours.

[0036] Optionally, the calcination temperature I is selected from any value of 400°C, 500°C, 600°C, 700°C, 800°C, 900°C or a range between any two of the above points.

[0037] Optionally, the calcination time I is selected from any value among 2h, 4h, 6h, 8h, 10h, 12h or a range value between any two of the above points.

[0038] Optionally, in step (2), the temperature of reaction II is 240-400° C., and the time of reaction II is 2-6 hours.

[0039] Optionally, the temperature of the reaction II is selected from any value of 240°C, 250°C, 300°C, 350°C, 400°C or a range between any two of the above points.

[0040] Optionally, the time of reaction II is selected from any value among 2h, 3h, 4h, 5h, 6h or a range between any two of the above points.

[0041] Optionally, the inert atmosphere is selected from at least one of a nitrogen atmosphere and an argon atmosphere.

[0042] Optionally, in step (3), the temperature of reaction III is 20 to 35° C., and the time of reaction III is 24 to 48 hours.

[0043] Optionally, the temperature of the reaction III is selected from any value of 20°C, 25°C, 30°C, 35°C, or a range between any two of the above points.

[0044] Optionally, the time of reaction III is selected from any value of 24h, 30h, 32h, 36h, 40h, 44h, 48h or a range between any two of the above points.

[0045] According to another aspect of the present application, there is provided a nitrogen / sulfur-modified activated carbon-supported single-atom noble metal catalyst prepared by the above-mentioned preparation method, and the use of the above-mentioned nitrogen / sulfur-modified activated carbon-supported single-atom noble metal catalyst in the preparation of methyl acetate.

[0046] Optionally, raw materials containing activated carbon-supported single-atom noble metal catalyst, methanol, a promoter, carbon monoxide, and hydrogen are reacted to obtain methyl acetate.

[0047] Optionally, the co-catalyst is methyl iodide.

[0048] Optionally, the mass ratio of the activated carbon-supported single-atom noble metal catalyst to the methanol is 1:1 to 1:10.

[0049] Optionally, the mass of the co-catalyst is 10-50% of the mass of the methanol.

[0050] Optionally, the volume ratio of H2 and CO is 0.01:1 to 2:1, and the gas flow rate is 40 to 100 mL / min.

[0051] Optionally, the reaction temperature is 160-240°C, the reaction pressure is 0.5-3.0 MPa, and the reaction liquid volume space velocity is 0.1-15 h -1 .

[0052] Optionally, the reaction temperature is selected from any value of 160°C, 170°C, 180°C, 190°C, 200°C, 220°C, 240°C or a range between any two of the above points.

[0053] Optionally, the reaction pressure is selected from any value among 0.5 MPa, 1 MPa, 1.5 MPa, 2 MPa, 2.5 MPa, 3.0 MPa or a range between any two of the above points.

[0054] Optionally, the liquid volume space velocity of the reaction is selected from 0.1h -1 , 1h -1 , 3h -1 , 5h -1 , 7h -1 , 9h -1 , 13h -1 , 15h -1 Any value in or a range of values ​​between the above two points.

[0055] In the present application, an activated carbon carrier is modified with nitrogen / sulfur and then treated with methyl iodide, and then coordinated with a noble metal precursor solution by a wet method to obtain a nitrogen / sulfur-modified activated carbon-supported single-atom noble metal catalyst.

[0056] In the present application, activated carbon and nitrogen / sulfur precursor are placed in a hydrothermal kettle for reaction, and then the solid is centrifuged and washed, and then vacuum dried and roasted, and the obtained black solid is modified activated carbon. The modified activated carbon is placed in a tubular furnace, and N2 is introduced and heated, and then iodomethane is bubbled and roasted to obtain modified activated carbon treated with iodomethane. The above-mentioned activated carbon is mixed and stirred with a noble metal precursor solution, and then dried after washing to obtain a nitrogen / sulfur-modified activated carbon-supported single-atom noble metal catalyst. The catalyst consists of two parts, a metal and a carrier, and the metal is one of Rh, Ru, Pd, Ir, Mo, Pt, and Ag, and the metal mass is 0.2-5.0wt.%, and the carrier is activated carbon. The catalyst is used in a fixed bed reactor, and at a certain temperature, pressure, and this catalyst, methanol and carbon monoxide can be efficiently converted into acetic acid and methyl acetate.

[0057] The beneficial effects of this application include:

[0058] 1) Compared with the prior art, the modified activated carbon carrier stably loaded with single-atom noble metal catalyst and the preparation method thereof of the present application are simple to operate, mild in conditions, and have strong universality.

[0059] 2) The method for modifying the carrier with controllable ligand configuration and stereoeffect developed in the present application optimizes the activated carbon-supported precious metal system by stably immobilizing the precious metal active species on the activated carbon in the form of coordination bonds, which requires the steps of achieving metal monodispersion through CO and methyl iodide, and replaces the polymer carrier with complex synthesis and insufficient stability, thereby reducing the reaction pressure and achieving efficient and stable catalytic carbonylation of methanol. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] Figure 1 This is the HAADF-STEM image of the single-atom Rh / AC-Thi catalyst 10 nm in Example 4 of the present application.

[0061] Figure 2 This is the HAADF-STEM image of the single-atom Rh / AC-Thi catalyst 2nm in Example 4 of the present application. DETAILED DESCRIPTION

[0062] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0063] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.

[0064] The present application adopts a fixed bed reactor to analyze the catalyst, the reactor material is Hastelloy C276, the tube length is 48cm, and the tube inner diameter is 6mm. After the reaction gas tail gas is cooled by a cold trap, the gas phase product is analyzed online by an Agilent 7890B gas chromatograph, a PQ packed column, and a TCD detector. After the liquid phase product is collected, it is analyzed offline by gas chromatography, a FFAP capillary column, and a FID detector. The analysis method is the internal standard method, and the internal standard is isobutanol.

[0065] The room temperature in the present application refers to 25°C.

[0066] In the examples of this application, the conversion rate and selectivity are calculated as follows:

[0067]

[0068]

[0069] The method for preparing the nitrogen / sulfur modified activated carbon supported single atom noble metal catalyst comprises the following steps:

[0070] Step 1: Place activated carbon and sulfur / nitrogen-sulfur precursor solution in a hydrothermal autoclave and treat at 150-180°C for 5-12h. After centrifugal washing, dry at 120°C, and calcine at 400-800°C in N2 atmosphere for 2-6h. The resulting black solid is sulfur / nitrogen-sulfur modified activated carbon; after mixing the activated carbon and nitrogen precursor evenly, place them in a tube furnace and treat at 600-900°C and N2 (30-100mL / min) for 5-12h. After centrifugal washing, dry at 120°C, and the resulting black solid is nitrogen-modified activated carbon. Among them, the mass ratio of nitrogen precursor melamine to activated carbon is 1:1-10:1; the mass ratio of sulfur precursor 2,2-bithiophene and 2-benzyl disulfide to activated carbon is 0.2:1-10:1; the mass ratio of nitrogen-sulfur precursor thiourea and thioacetamide to activated carbon is 0.2:1-5:1.

[0071] Step 2: Place the modified activated carbon obtained in step 1 in a tubular furnace, introduce N2 (30-50 mL / min) and heat to 240-400°C, then bubble iodomethane into the furnace and roast for 2-6 hours to obtain modified activated carbon treated with iodomethane.

[0072] Step 3: Mix the activated carbon in step 2 with the noble metal precursor solution, stir at room temperature for 24 to 48 hours, wash and dry at 120° C. to obtain a nitrogen / sulfur-modified activated carbon-supported single-atom noble metal catalyst.

[0073] 0.25 g of the catalyst prepared in this application was loaded into a Harbin alloy fixed bed reactor, the reaction temperature was 160-240°C, the reaction pressure was 0.5-3.0 MPa, and the reaction liquid volume space velocity was 0.1-15 h -1The mass of the co-catalyst methyl iodide is 10-50% of the mass of the methanol, and the volume ratio of H2 and CO is 0.01:1-2:1.

[0074] Example 1

[0075] 1.0g activated carbon and 1.0g 2,2-bithiophene aqueous solution (40mL) were mixed evenly and placed in a hydrothermal autoclave. The solution was treated at 150℃ for 6h. The solid from the above reaction was washed with deionized water by centrifugation and dried at 120℃. It was calcined at 400℃ in N2 atmosphere for 4h. The obtained black solid was sulfur-modified activated carbon, which was marked as AC-DBDS. AC-DBDS was placed in a tubular furnace, N2 (30mL / min) was introduced and the temperature was raised to 300℃, and then iodomethane was bubbled in. Under this condition, it was calcined for 4h to obtain modified activated carbon treated with iodomethane, which was marked as AC-DBDS-I.

[0076] 1.0 g AC-DBDS-I was mixed with 30 mL of a dichloromethane solution of carbonyl rhodium chloride dimer, wherein the mass percentage of Rh was 1%, and stirred at room temperature for 20 h. After washing with dichloromethane, the mixture was dried at 120° C. to obtain a sulfur-modified activated carbon-supported single-atom Rh catalyst, which was labeled as Rh / AC-DBDS.

[0077] Example 2

[0078] 1.0g activated carbon and 1.0g 2-benzyl disulfide aqueous solution (40mL) were mixed evenly and placed in a hydrothermal autoclave, and the solution was treated at 150℃ for 6h. The solid from the above reaction was washed with deionized water by centrifugation and dried at 120℃, and calcined at 400℃ in N2 atmosphere for 4h. The obtained black solid was sulfur-modified activated carbon, marked as AC-BPT. AC-BPT was placed in a tubular furnace, N2 (30mL / min) was introduced and the temperature was raised to 300℃, and then iodomethane was bubbled in. Under this condition, iodomethane-treated modified activated carbon was obtained, marked as AC-BPT-I.

[0079] 1.0 g AC-BPT-I was mixed with 30 mL of a dichloromethane solution of carbonyl rhodium chloride dimer, wherein the mass percentage of Rh was 1%, and stirred at room temperature for 20 h. After washing with dichloromethane, the mixture was dried at 120° C. to obtain a sulfur-modified activated carbon-supported single-atom Rh catalyst, which was labeled as Rh / AC-BPT.

[0080] Example 3

[0081] 0.5g activated carbon and 2.5g melamine solid were mixed thoroughly and placed in a tube furnace, N2 atmosphere 50mL / min, 2℃ / min to 800℃, and maintained for 4h. The resulting black solid was nitrogen-modified activated carbon, marked as AC-N. AC-N was placed in a tube furnace, N2 (30mL / min) was introduced and the temperature was raised to 300℃, and then iodomethane was bubbled in. Under this condition, calcination for 4h was obtained to obtain iodomethane-treated modified activated carbon, marked as AC-NI.

[0082] 1.0 g AC-NI was mixed with 30 mL of a dichloromethane solution of carbonyl rhodium chloride dimer, wherein the mass percentage of Rh was 1%, and stirred at room temperature for 20 h. After washing with dichloromethane, the mixture was dried at 120° C. to obtain a nitrogen-modified activated carbon-supported single-atom Rh catalyst, which was labeled as Rh / AC-N.

[0083] Example 4

[0084] 0.5g activated carbon was mixed with 0.5g thiourea aqueous solution (20mL) and placed in a hydrothermal autoclave. The solution was treated at 180℃ for 8h. The solid from the above reaction was washed with deionized water by centrifugation and dried at 120℃. It was calcined at 400℃ in N2 atmosphere for 4h. The obtained black solid was sulfur-modified activated carbon, which was marked as AC-Thi. AC-Thi was placed in a tubular furnace, N2 (30mL / min) was introduced and the temperature was raised to 240℃, and then iodomethane was bubbled in. Under this condition, it was calcined for 4h to obtain modified activated carbon treated with iodomethane, which was marked as AC-Thi-I.

[0085] 0.5 g AC-Thi-I was mixed with 20 mL of a solution of carbonyl rhodium chloride dimer in which the mass percentage of Rh was 1%, stirred at room temperature for 24 h, washed with dichloromethane and dried at 120 °C to obtain a nitrogen-sulfur co-modified activated carbon-supported single-atom Rh catalyst, labeled as Rh / AC-Thi.

[0086] from Figure 1 It can be seen that no obvious metal particles were observed in the prepared Rh / AC-Thi catalyst, indicating that the Rh metal is evenly dispersed on the support surface.

[0087] from Figure 2 It can be seen that evenly dispersed Rh can be observed under a high-power electron microscope, indicating that Rh is evenly dispersed on the carrier surface in the form of single atoms.

[0088] Example 5

[0089] 0.5g activated carbon and 0.5g thioacetamide aqueous solution (20mL) were mixed evenly and placed in a hydrothermal autoclave, and the solution was treated at 180℃ for 8h. The solid from the above reaction was washed with deionized water by centrifugation and dried at 120℃, and calcined at 400℃ in N2 atmosphere for 4h. The obtained black solid was sulfur-modified activated carbon, which was marked as AC-TAA. AC-TAA was placed in a tubular furnace, N2 (30mL / min) was introduced and the temperature was raised to 240℃, and then iodomethane was bubbled in. Under this condition, iodomethane was calcined for 4h to obtain modified activated carbon treated with iodomethane, which was marked as AC-TAA-I.

[0090] 0.5 g AC-TAA-I was mixed with 20 mL of a solution of carbonyl rhodium chloride dimer, in which the mass percentage of Rh was 1%, and stirred at room temperature for 24 h. After washing with dichloromethane, the mixture was dried at 120° C. to obtain a nitrogen-sulfur co-modified activated carbon-supported single-atom Rh catalyst, which was labeled as Rh / AC-TAA.

[0091] Example 6

[0092] 0.5g activated carbon was mixed with 0.5g thiourea aqueous solution (20mL) and placed in a hydrothermal autoclave. The solution was treated at 180℃ for 8h. The solid from the above reaction was washed with deionized water by centrifugation and dried at 120℃. It was calcined at 400℃ in N2 atmosphere for 4h. The obtained black solid was sulfur-modified activated carbon, which was marked as AC-Thi. AC-Thi was placed in a tubular furnace, N2 (30mL / min) was introduced and the temperature was raised to 240℃, and then iodomethane was bubbled in. Under this condition, it was calcined for 4h to obtain modified activated carbon treated with iodomethane, which was marked as AC-Thi-I.

[0093] 0.5 g AC-Thi-I was mixed with 20 mL of a dichloromethane solution of ruthenium hexacarbonyl chloride, in which the mass percentage of Ru was 1%, and stirred at room temperature for 48 h. After washing with dichloromethane, the mixture was dried at 120° C. to obtain a nitrogen-sulfur co-modified activated carbon-supported single-atom Ru catalyst, which was labeled as Ru / AC-Thi.

[0094] Example 7

[0095] 0.5g activated carbon was mixed with 0.5g thiourea aqueous solution (20mL) and placed in a hydrothermal autoclave. The solution was treated at 180℃ for 8h. The solid from the above reaction was washed with deionized water by centrifugation and dried at 120℃. It was calcined at 400℃ in N2 atmosphere for 4h. The obtained black solid was sulfur-modified activated carbon, which was marked as AC-Thi. AC-Thi was placed in a tubular furnace, N2 (30mL / min) was introduced and the temperature was raised to 240℃, and then iodomethane was bubbled in. Under this condition, it was calcined for 4h to obtain modified activated carbon treated with iodomethane, which was marked as AC-Thi-I.

[0096] 0.5 g AC-Thi-I was mixed with 20 mL of a dichloromethane solution of iridium dicarbonyl acetylacetonate, in which the mass percentage of Ir was 1%, and stirred at room temperature for 30 h. After washing with dichloromethane, the mixture was dried at 120° C. to obtain a nitrogen-sulfur co-modified activated carbon-supported single-atom Ir catalyst, which was labeled as Ir / AC-Thi.

[0097] Example 8

[0098] 0.5g activated carbon was mixed with 0.5g thiourea aqueous solution (20mL) and placed in a hydrothermal autoclave. The solution was treated at 180℃ for 8h. The solid from the above reaction was washed with deionized water by centrifugation and dried at 120℃. It was calcined at 400℃ in N2 atmosphere for 4h. The obtained black solid was sulfur-modified activated carbon, which was marked as AC-Thi. AC-Thi was placed in a tubular furnace, N2 (30mL / min) was introduced and the temperature was raised to 240℃, and then iodomethane was bubbled in. Under this condition, it was calcined for 4h to obtain modified activated carbon treated with iodomethane, which was marked as AC-Thi-I.

[0099] 0.5 g AC-Thi-I was mixed with 20 mL of chloroplatinic acid aqueous solution, in which the mass percentage of Pt was 3%, stirred at room temperature for 24 h, washed with deionized water and dried at 120 ° C to obtain a nitrogen-sulfur co-modified activated carbon-supported single-atom Pt catalyst, marked as Pt / AC-Thi.

[0100] Example 9

[0101] 0.5g activated carbon was mixed with 0.5g thiourea aqueous solution (20mL) and placed in a hydrothermal autoclave. The solution was treated at 180℃ for 8h. The solid from the above reaction was washed with deionized water by centrifugation and dried at 120℃. It was calcined at 400℃ in N2 atmosphere for 4h. The obtained black solid was sulfur-modified activated carbon, which was marked as AC-Thi. AC-Thi was placed in a tubular furnace, N2 (30mL / min) was introduced and the temperature was raised to 240℃, and then iodomethane was bubbled in. Under this condition, it was calcined for 4h to obtain modified activated carbon treated with iodomethane, which was marked as AC-Thi-I.

[0102] 0.5 g AC-Thi-I was mixed with 20 mL of a tetrahydrofuran solution of palladium chloride, wherein the mass percentage of Pd was 1%, and stirred at room temperature for 48 h. After washing with tetrahydrofuran, the mixture was dried at 120° C. to obtain a nitrogen-sulfur co-modified activated carbon-supported single-atom Pd catalyst, which was labeled as Pd / AC-Thi.

[0103] Example 10

[0104] 0.5g activated carbon was mixed with 0.5g thiourea aqueous solution (20mL) and placed in a hydrothermal autoclave. The solution was treated at 180℃ for 8h. The solid from the above reaction was washed with deionized water by centrifugation and dried at 120℃. It was calcined at 400℃ in N2 atmosphere for 4h. The obtained black solid was sulfur-modified activated carbon, which was marked as AC-Thi. AC-Thi was placed in a tubular furnace, N2 (30mL / min) was introduced and the temperature was raised to 240℃, and then iodomethane was bubbled in. Under this condition, it was calcined for 4h to obtain modified activated carbon treated with iodomethane, which was marked as AC-Thi-I.

[0105] 0.5 g AC-Thi-I was mixed with 20 mL of a dichloromethane solution of molybdenum acetylacetonate, wherein the mass percentage of Mo was 0.5%, and stirred at room temperature for 24 h. After washing with dichloromethane, the mixture was dried at 120° C. to obtain a nitrogen-sulfur co-modified activated carbon-supported single-atom Mo catalyst, which was labeled as Mo / AC-Thi.

[0106] Embodiment 11

[0107] 0.5g activated carbon was mixed with 0.5g thiourea aqueous solution (20mL) and placed in a hydrothermal autoclave. The solution was treated at 180℃ for 8h. The solid from the above reaction was washed with deionized water by centrifugation and dried at 120℃. It was calcined at 400℃ in N2 atmosphere for 4h. The obtained black solid was sulfur-modified activated carbon, which was marked as AC-Thi. AC-Thi was placed in a tubular furnace, N2 (30mL / min) was introduced and the temperature was raised to 240℃, and then iodomethane was bubbled in. Under this condition, it was calcined for 4h to obtain modified activated carbon treated with iodomethane, which was marked as AC-Thi-I.

[0108] 0.5 g AC-Thi-I was mixed with 20 mL of silver nitrate aqueous solution, in which the mass percentage of Ag was 1%, stirred at room temperature for 30 h, washed with deionized water and dried at 120 °C to obtain a nitrogen-sulfur co-modified activated carbon-supported single-atom Ag catalyst, marked as Ag / AC-Thi.

[0109] Example 12

[0110] The catalysts prepared in the above application case examples 1 to 11 were used in the reaction of preparing methyl acetate with methanol and CO as raw materials respectively.

[0111] The carbonylation reaction conditions are as follows: catalyst dosage 0.25 g, reaction temperature 200 ° C, reaction pressure 1.7 MPa, methyl iodide to methanol mass ratio = 7:3, liquid feed 0.1 mL / min, H2 and CO volume ratio 1:10, gas flow rate 60 mL / min. After the reaction gas tail gas is cooled by a cold trap, the gas phase product is analyzed online by an Agilent 7890B gas chromatograph, PQ packed column, TCD detector. After the liquid phase product is collected, it is analyzed offline by gas chromatography, FFAP capillary column, FID detector, and the analysis method is the internal standard method, and the internal standard is isobutanol.

[0112] Using the catalyst prepared in Example 1-11, methyl acetate was prepared according to the above operation. The methanol conversion rate and methyl acetate selectivity are shown in Table 1.

[0113]

[0114]

[0115] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A nitrogen / sulfur modified activated carbon supported single atom noble metal catalyst, characterized in that: The activated carbon-supported single-atom noble metal catalyst comprises a noble metal, a non-metal, and a carrier; The noble metal and the non-metal are immobilized on the carrier; The noble metal is selected from at least one of Rh, Ru, Pd, Ir, Mo, Pt and Ag; The non-metal is nitrogen and / or sulfur; The carrier is activated carbon.

2. The activated carbon-supported single-atom noble metal catalyst according to claim 1, characterized in that: The mass of the noble metal is 0.2 to 5.0 wt.% of the mass of the activated carbon-supported single-atom noble metal catalyst.

3. The method for preparing an activated carbon-supported single-atom noble metal catalyst according to any one of claims 1 to 2, characterized in that: The preparation method comprises the following steps: (1) reacting a mixture I containing activated carbon and a nitrogen / sulfur precursor solution, drying I, and calcining I to obtain nitrogen / sulfur modified activated carbon; (2) reacting the nitrogen / sulfur modified activated carbon with methyl iodide under an inert atmosphere to obtain methyl iodide modified activated carbon; (3) reacting a mixture II containing iodomethane-modified activated carbon and a noble metal precursor solution, and drying III to obtain a nitrogen / sulfur-modified activated carbon-supported single-atom noble metal catalyst.

4. The preparation method according to claim 3, characterized in that: The nitrogen / sulfur precursor solution is selected from at least one of a nitrogen precursor solution, a sulfur precursor solution, and a nitrogen-sulfur precursor solution; Preferably, the nitrogen precursor solution is melamine; Preferably, the sulfur precursor solution is selected from 2,2-bithiophene and / or 2-benzyl disulfide; Preferably, the nitrogen-sulfur precursor solution is selected from thiourea and / or thioacetamide.

5. The preparation method according to claim 4, characterized in that: The mass ratio of the nitrogen precursor solution to the activated carbon is 1:1 to 10:1; Preferably, the mass ratio of the sulfur precursor to the activated carbon is 0.2:1 to 10:1; Preferably, the mass ratio of the nitrogen-sulfur precursor to the activated carbon is 0.2:1 to 5:

1.

6. The preparation method according to claim 3, characterized in that: The noble metal precursor solution is selected from at least one of carbonyl rhodium chloride dimer, hexacarbonyl ruthenium chloride, dicarbonyl iridium acetylacetonate, chloroplatinic acid, palladium chloride, molybdenum acetylacetonate, and silver nitrate; Preferably, the mass ratio of the nitrogen / sulfur modified activated carbon to methyl iodide is 1:10 to 1:50; Preferably, the mass ratio of the iodomethane-modified activated carbon to the noble metal precursor solution is 1:5 to 1:

20.

7. The preparation method according to claim 3, characterized in that: In the step (1), the temperature of the reaction I is 150 to 180° C., and the reaction time is 5 to 12 hours; Preferably, the temperature of the drying I is 80 to 150° C., and the drying I time is 12 to 24 hours; Preferably, the temperature of the calcination I is 400-900° C., and the time of the calcination I is 2-12 hours. Preferably, in step (2), the temperature of reaction II is 240-400° C., and the time of reaction II is 2-6 h; Preferably, the inert atmosphere is selected from at least one of a nitrogen atmosphere and an argon atmosphere; Preferably, in step (3), the temperature of reaction III is 20 to 35° C., and the time of reaction III is 24 to 48 hours.

8. Use of the activated carbon-supported single-atom noble metal catalyst according to any one of claims 1 to 2 or the activated carbon-supported single-atom noble metal catalyst prepared by the preparation method according to any one of claims 3 to 7 in the preparation of methyl acetate.

9. The use according to claim 8, characterized in that: reacting a raw material containing an activated carbon-supported single-atom noble metal catalyst, methanol, a promoter, carbon monoxide, and hydrogen to obtain methyl acetate; Preferably, the co-catalyst is methyl iodide; Preferably, the mass ratio of the activated carbon-supported single-atom noble metal catalyst to the methanol is 1:1 to 1:10; Preferably, the mass of the co-catalyst is 10-50% of the mass of the methanol; Preferably, the volume ratio of H2 to CO is 0.01:1 to 2:1, and the gas flow rate is 40 to 100 mL / min.

10. The use according to claim 9, characterized in that: The reaction temperature is 160-240°C, the reaction pressure is 0.5-3.0 MPa, and the reaction liquid volume space velocity is 0.1-15 h -1 .

Citation Information

Patent Citations

  • Monatomic noble metal catalyst, preparation method thereof and application thereof in room-temperature catalytic oxidation of formaldehyde

    CN109939712A

  • Biomass activated carbon-loaded metal monoatomic catalyst and preparation and application thereof

    CN110026186A

  • Monoatomically dispersed noble metal catalyst and preparation method and application thereof

    CN111195515A

  • Atomic-scale monodispersed rhodium-based catalyst, preparation method thereof and application of atomic-scale monodispersed rhodium-based catalyst in preparation of methyl acetate through methanol gas-phase carbonylation

    CN111195516A

  • Porous carbon-loaded monatomic metal nitrogen coordination composite material and preparation method thereof

    CN111620311A