Preparation method and application of three-dimensional continuous porous carbon loaded lamellar iron-based sulfide
Through three-dimensional continuous porous carbon-loaded sheet-like iron-based sulfide catalyst, the limitations of traditional Fenton technology under acidic conditions and the generation of iron sludge are solved, and the efficient degradation of various pollutants under natural pH conditions is achieved. It is carbamazepine and other organic pollutants, and has strong anti-interference and stability.
Patent Information
- Application Number
- CN202410833406.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional homogeneous Fenton technology can only be performed under acidic conditions, producing a large amount of iron sludge, slow Fe2+ regeneration, limiting its large-scale application and difficult to effectively remove a variety of pollutants, especially under natural pH conditions.
Using a three-dimensional continuous porous carbon-loaded sheet layered iron-based sulfide catalyst, it is prepared by two steps of hydrothermal preparation to form a layered structure, which can effectively degrade a variety of pollutants under natural pH conditions, including ciprofloxacin, parachlorophenol and Bisphenol A and remove antibiotic wastewater within a wide pH range.
Under natural pH ≈7.0, the H2O2 addition amount is 3mM and the catalyst is 0.1g/L, the pollutant degradation rate within 120 minutes can reach 98.7%, and it has strong anti-interference ability, which can efficiently remove Kama under alkaline conditions. Xiping, and the catalyst maintains high activity during recycling.
Smart Images

Figure CN118904359A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of advanced oxidation technology treatment, and specifically relates to a preparation method and application of three-dimensional continuous porous carbon-loaded lamellar iron-based sulfide. Background Art
[0002] The emergence of emerging pollutants has seriously endangered the water environment and human safety. Advanced oxidation technology is considered to be an effective wastewater treatment technology that can effectively remove harmful pollutants in water. Among them, the Fenton reaction has attracted widespread attention because it can produce a large number of free radicals, attack pollutants indiscriminately, and effectively decompose organic pollutants into CO2 and H2O, thereby reducing the harm of organic pollutants and the biodegradability of difficult-to-degrade pollutants. However, the traditional homogeneous Fenton technology (Fe 2+ / H2O2) can only be carried out under acidic conditions, and a large amount of iron sludge will be produced, and the slow Fe 2+ Regeneration, etc., is not conducive to the production of active species, thus limiting its large-scale application.
[0003] However, heterogeneous Fenton technology can effectively overcome the shortcomings of traditional homogeneous Fenton technology and become an alternative technology. Because it can broaden the pH range, reduce the generation of iron sludge and effectively promote Fe 3+ / Fe 2+ cycle, which has attracted the attention of many researchers. Summary of the invention
[0004] In view of the deficiencies of the prior art, the purpose of the present invention is to provide a preparation method and application of a three-dimensional continuous porous carbon-supported lamellar iron-based sulfide. The present invention utilizes a catalyst to activate H2O2 to remove refractory organic pollutants in water. The Fenton-like system constructed by the present invention greatly improves the treatment efficiency of wastewater. Under the conditions of natural pH≈7.0, H2O2 dosage of 3mM, and catalyst dosage of 0.1g / L, the pollutant degradation rate within 120min can reach 98.7%, and it can adapt to the removal of various pollutants (including ciprofloxacin (CIP), parachlorophenol (4-CP), bisphenol A (BPA)), has strong anti-interference ability, and can effectively remove antibiotic wastewater (containing carbamazepine-contaminated water) in a wide pH range. At the same time, the preparation method of the porous structure-modified iron-based catalyst is described.
[0005] A method for preparing three-dimensional continuous porous carbon-supported lamellar iron-based sulfide comprises the following steps:
[0006] 1) Add N-containing porous carbon to deionized water, add Fe salt after ultrasonic homogenization, stir vigorously to make Fe ions fully dispersed in the solution, then transfer the mixture to a high-pressure reactor, heat the high-pressure reactor in a sealed state to obtain porous carbon-loaded FeOOH, recorded as NCF;
[0007] 2) adding the NCF and thioacetamide to ethylene glycol, stirring sufficiently, transferring the reaction mixture to a high-pressure reactor, sealing the high-pressure reactor for heating reaction, washing and drying after the reaction, and preparing the three-dimensional continuous porous carbon-supported lamellar iron-based sulfide.
[0008] Furthermore, in step 1), the feed ratio of the N-containing porous carbon to the Fe salt is 2-6 mg:1 mmol, preferably 4-4.5 mg:1 mmol, and the dispersion concentration of the N-containing porous carbon in deionized water is 0.5-2 mg / mL, preferably 0.8-1 mg / mL.
[0009] Furthermore, in step 1), the reaction temperature is 85-90° C. and the reaction time is 10-15 h.
[0010] Furthermore, in step 2), the mass ratio of NCF to thioacetamide is 1:1-10, preferably 1:3-10, and the dispersion concentration of NCF in ethylene glycol is 0.5-2 mg / mL, preferably 1-1.25 mg / mL.
[0011] Furthermore, in step 2), the reaction temperature is 130-140° C., and the reaction time is 6-10 h.
[0012] Furthermore, the preparation method of the N-containing porous carbon in step 1) is: melamine and sodium citrate are mixed in a mass ratio of 0.5-2:10 and fully ground, and then calcined at 600-800°C for 1-4h under an inert atmosphere, and the calcined product is stirred in a 3-5M HCl solution for 20-30h, and then the HCl solution is removed by filtration, and washed with deionized water several times until the pH of the eluent is close to neutral, and finally filtered and dried to obtain the N-containing porous carbon.
[0013] In the preparation process of the catalyst material of the present invention, sodium citrate is used as a carbon source, and finally, after carbonization, acid washing is performed to remove sodium ions, so that three-dimensional continuous porous carbon can be well formed. In addition, melamine is used as a nitrogen source, which is beneficial to improving the loading effect of Fe salt on the one hand, and regulating the electronic structure of the catalyst on the other hand, thereby improving the catalytic activity.
[0014] Furthermore, the mass ratio of melamine to sodium citrate is 1-1.2:10, and the roasting temperature is 700-750°C.
[0015] The present invention also provides the use of the three-dimensional continuous porous carbon-supported lamellar iron-based sulfide in catalytic degradation of antibiotic-contaminated water. The catalytic degradation is carried out using a Fenton catalytic system. A catalyst with a final concentration of 0.08-0.1 g / L and 2-4 mM H2O2 are added to the antibiotic-contaminated water, and a catalytic degradation reaction is carried out at a pH of 4-9.
[0016] In a first aspect, the present invention provides a three-dimensional continuous porous carbon-supported lamellar iron-based sulfide composite nanomaterial having a layered structure, and the material is obtained by two-step hydrothermal treatment.
[0017] Preferably, melamine is used as the nitrogen functional group source to better anchor the iron ions.
[0018] In a second aspect, the present invention provides the use of the aforementioned three-dimensional continuous porous carbon-loaded lamellar iron-based sulfide material in degrading antibiotic-contaminated water.
[0019] Preferably, the antibiotic compound is carbamazepine.
[0020] Compared with the prior art, the present invention has the following advantages:
[0021] 1. The present invention uses three-dimensional continuous porous carbon to load lamellar iron-based sulfide materials, which can activate H2O2 to effectively degrade carbamazepine (CBZ); and, compared with other materials, the continuous porous carbon / Fe3S4@FeS2 of the present invention can also remove other pollutants, such as parachlorophenol, ciprofloxacin, and bisphenol A.
[0022] 2. The three-dimensional continuous porous carbon-supported lamellar iron-based sulfide material provided by the present invention can self-adjust the pH of the reaction solution to acidity, avoiding additional acid adjustment, and can also achieve efficient removal of carbamazepine under alkaline conditions (pH=10).
[0023] 3. The three-dimensional continuous porous carbon-supported lamellar iron-based sulfide material provided by the present invention has iron-based sulfide components of Fe3S4 and FeS2, and the low-valent sulfur species contained in it can not only provide electrons to promote Fe 3+ / Fe 2+ It can not only effectively reduce the instability of sulfides, but also avoid the leaching of iron ions and the loss of low-valent sulfur species.
[0024] 4. The present invention uses three-dimensional continuous porous carbon-supported lamellar iron-based sulfide materials in the degradation of CBZ in water, and HO· is the core active substance. Therefore, the degradation of CBZ is less affected by different anions and cations and natural organic matter, except for HCO3 - and H2PO4 - Can react with HO· to produce weak HCO3- ·H2PO4 - In addition to its great impact, it has a good application prospect in remediating pollutants in water bodies. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a SEM image of the three-dimensional continuous porous carbon-supported lamellar iron-based sulfide material prepared under the conditions of TAA:NCF=3:1 in Example 1 of the present invention.
[0026] Figure 2 These are the XRD patterns of pure continuous porous carbon, NCF, and three-dimensional continuous porous carbon-supported lamellar iron-based sulfide materials with mass ratios of TAA:NCF=10:1, 5:1, 3:1, and 1:1 according to Example 1 of the present invention.
[0027] Figure 3 The CBZ degradation of different materials of the present invention within 120 min under the conditions of natural pH≈7.0, H2O2 dosage of 3 mM, and catalyst dosage of 0.1 g / L.
[0028] Figure 4 The figure shows the degradation of CBZ by the material of the present invention (TAA:NCF=3:1) under different pH conditions.
[0029] Figure 5 The figure shows the degradation of CBZ by the material of the present invention (TAA:NCF=3:1) under the number of cycles.
[0030] Figure 6 This is the degradation of 4-CP, CIP and BPA by the material prepared in Example 1 of the present invention (TAA:NCF=3:1) at pH≈7.0.
[0031] Figure 7 This is the degradation of CBZ by the material prepared in Example 1 of the present invention (TAA:NCF=3:1) under the influence of different background ions. DETAILED DESCRIPTION
[0032] The present invention will be further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0033] Unless otherwise stated, all materials and reagents used were obtained from commercial channels.
[0034] Example 1
[0035] A three-dimensional continuous porous carbon-supported lamellar iron-based sulfide heterogeneous Fenton catalyst uses continuous porous carbon as a carrier to prepare three-dimensional continuous porous carbon-supported oxyhydroxide iron (NCF), which is then sulfided to form a three-dimensional continuous porous carbon-supported lamellar iron-based sulfide with a layered morphology.
[0036] The preparation method of the three-dimensional continuous porous carbon-supported lamellar iron-based sulfide material comprises the following steps:
[0037] Step 1: Weigh 1.0g of melamine and 10.0g of sodium citrate in a mortar and grind them thoroughly. Then, in an argon atmosphere, heat the mixture to 700°C at a heating rate of 5°C / min and calcine at a constant temperature for 2h. After calcination, disperse the product in a 4M HCl solution and stir for 24h, then filter to remove the HCl solution and wash with deionized water several times until the eluent is close to a neutral pH. Finally, filter and dry at 80°C for 12h to obtain a three-dimensional continuous porous carbon.
[0038] Step 2: Weigh 40 mg of the synthesized three-dimensional continuous porous carbon and place it in 50 mL of deionized water, and ultrasonicate for 2 hours to fully disperse it. Subsequently, add 1.98 g of FeCl2·4H2O to the solution, stir vigorously for 1 hour, and then transfer the mixture to a 100 mL Teflon-lined steel autoclave, seal the autoclave, heat to 90°C, and keep it at this temperature for 12 hours. After natural cooling, filter and recover the precipitate, and wash it with deionized water 3 times. Finally, the material is dried in a vacuum oven at 60°C to obtain NCF.
[0039] Step 3, weigh 50 mg of pre-prepared NCF and thioacetamide (TAA) in different weight ratios (1:1, 1:3, 1:5, 1:10), add to 40 mL of ethylene glycol, stir for 0.5 h, transfer the reaction mixture to a 100 ml Teflon-lined steel autoclave, seal the autoclave, and keep it at 140 ° C for 8 h. Finally, wash three times with deionized water and anhydrous ethanol, and then vacuum dry at 60 ° C for 12 h. According to the above method, three-dimensional continuous porous carbon-supported lamellar iron-based sulfide materials with mass ratios of TAA: NCF = 10:1, 5:1, 3:1 and 1:1 were prepared respectively.
[0040] Example 1 SEM image of three-dimensional continuous porous carbon-supported lamellar iron-based sulfide material prepared under the condition of TAA: NCF = 3:1 Figure 1 As shown, it can be seen that the catalyst as a whole is a porous carbon network supported lamellar iron-based sulfide structure.
[0041] XRD analysis of pure continuous porous carbon, NCF and three-dimensional continuous porous carbon supported lamellar iron-based sulfide materials with mass ratios of TAA:NCF = 10:1, 5:1, 3:1 and 1:1 is shown in Figure 2. Figure 2 As shown, it was found that the continuous porous carbon had a graphitic carbon structure, and the three-dimensional continuous porous carbon supported lamellar iron-based sulfides containing Fe3S4 and FeS2.
[0042] Example 2
[0043] The method for removing CBZ from water is as follows: the catalyst prepared in Example 1 is added to the water to be treated, and the treated water is deionized water containing carbamazepine pollutants, and the following experiment is performed:
[0044] The test was performed in a 150 mL serum bottle containing 100 mL of CBZ solution (10 mg L -1 ). Use 0.1MNaOH and H2SO4 to adjust the required pH. Subsequently, add a predetermined amount of catalyst and a specific concentration of H2O2. Place the serum bottle on a constant temperature shaker (250rpm, 25°C) and carry out catalytic degradation reaction under the conditions of natural pH≈7.0, a final concentration of H2O2 of 3mM, and a catalyst dosage of 0.1g / L. Use a 1ml syringe to draw samples from the serum bottle at regular intervals, quench the reaction with 20μL of n-butanol, and then filter with a 0.22μm polytetrafluoroethylene filter for subsequent analysis. In order to ensure the reliability of the experiment, each experiment was performed three times.
[0045] According to the above experimental conditions, the three-dimensional continuous porous carbon-supported lamellar iron-based sulfide material prepared under the mass ratio of TAA:NCF=10:1, 5:1, 3:1 and 1:1 in Example 1 was used as the catalyst. The catalytic degradation results at different times are shown in Figure 3 The degradation performance of continuous porous carbon / Fe3S4@FeS2 materials with different ratios on CBZ was evaluated. Figure 3 It can be seen that when the mass ratio TAA:NCF=3:1, the three-dimensional continuous porous carbon-loaded lamellar iron-based sulfide material has the best Fenton-like reaction performance and can be used as a material for the degradation of pollutants in water with excellent performance.
[0046] According to the above experimental conditions, the three-dimensional continuous porous carbon-supported lamellar iron-based sulfide material prepared under the conditions of TAA:NCF=3:1 in Example 1 was used as a catalyst. The catalytic degradation results at different pH and different time are shown in Figure 4 It can be seen that the material has higher catalytic activity under acidic conditions, and it can also be seen that the material can still remove CBZ well even under alkaline conditions.
[0047] The three-dimensional continuous porous carbon-supported lamellar iron-based sulfide material provided in Example 1 was used for recycling to evaluate the stability of the material. The specific operation was as follows: according to the above experimental conditions, the catalyst was filtered and recovered every 100 minutes of catalytic degradation operation, and after vacuum drying at 60°C, it was put into the next batch of catalytic degradation system for repeated application of the catalyst. The three-dimensional continuous porous carbon-supported lamellar iron-based sulfide material prepared under the conditions of TAA:NCF=3:1 in Example 1 was used as the catalyst. The degradation of CBZ under different recycling times of the catalyst was shown in Figure 5 .from Figure 5 It can be seen that the material still maintains a high catalytic activity after four consecutive runs, and the removal rate of CBZ can still reach 88.7%, which shows that the material has good stability. In addition, the degradation of CBZ is less affected by different anions and natural organic matter, except for HCO3 - and H2PO4 - Can react with HO· to produce weak HCO3 - ·H2PO4 - In addition to its great impact, it has a good application prospect in remediating pollutants in water bodies.
[0048] Example 3
[0049] The comparative experiment of using the three-dimensional continuous porous carbon-supported lamellar iron-based sulfide material provided in Example 1 to decompose different pollutants (parachlorophenol, ciprofloxacin or bisphenol A) is as follows:
[0050] Take 10mL of 100mg / L pollutant solution and 90mL of deionized water in a 150mL serum bottle, then add 10mg of the three-dimensional continuous porous carbon-supported lamellar iron-based sulfide material prepared under the conditions of TAA:NCF=3:1 in Example 1 as a catalyst, and then add a specific concentration of H2O2. The serum bottle was placed on a constant temperature shaker (250rpm, 25℃), and the catalytic degradation reaction was carried out under the conditions of natural pH≈7.0, the final concentration of H2O2 added was 3mM, and the amount of catalyst added was 0.1g / L. Samples were drawn from the serum bottle at regular intervals with a 1ml syringe, the reaction was quenched with 20μL of n-butanol, and then filtered with a 0.22μm polytetrafluoroethylene filter for subsequent analysis. In order to ensure the reliability of the experiment, each experiment was performed three times.
[0051] Three experimental groups were set up; the pollutants used in the three experiments were p-chlorophenol, ciprofloxacin and bisphenol A; the results of the degradation of 4-CP, CIP and BPA were shown in Figure 6 shown; from Figure 6 It can be seen that the three-dimensional continuous porous carbon-supported lamellar iron-based sulfide material provided in Example 1 has a good removal effect on different pollutants.
[0052] Example 4
[0053] The three-dimensional continuous porous carbon-supported lamellar iron-based sulfide material provided in Example 1 was used cyclically to evaluate the material's anti-interference ability to background ions. The specific operation is as follows:
[0054] Take 10mL of 100mg / L CBZ solution and 90mL of deionized water in a 150mL serum bottle, and then add 0.5mL of background ion solution (1mol / L), except for 10mg / L of humic acid. Subsequently, add a predetermined amount of catalyst and a specific concentration of H2O2. Place the serum bottle on a constant temperature shaker (250rpm, 25℃), and carry out catalytic degradation reaction under the conditions of natural pH≈7.0, a final concentration of H2O2 of 3mM, and a catalyst dosage of 0.1g / L. Use a 1ml syringe to extract samples from the serum bottle at regular intervals, quench the reaction with 20μL of n-butanol, and then filter with a 0.22μm polytetrafluoroethylene filter for subsequent analysis. The specific effects are as follows: Figure 7 As shown, it shows that the material has a certain anti-interference ability.
[0055] Figure 7 A curve in the figure corresponds to a set of interference experiments of background ions. Each set of experiments was conducted under the conditions of "degradation of CBZ within 120 min at natural pH ≈ 7.0, 3 mM H2O2 dosage, and 0.1 g / L catalyst dosage". The interference substances in each experimental group correspond to Figure 7 The substances on the corresponding curves, i.e., the interfering ions, are Cl with a final concentration of 5 mmol / L. - 、NO3 - 、SO4 2- 、HCO3 - 、H2PO4 - (The cations combined with the anions are all Na + ) and humic acid at a final concentration of 10 mg / L.
[0056] The contents described in this specification are merely an enumeration of implementation forms of the inventive concept, and the protection scope of the present invention should not be regarded as being limited to the specific forms described in the embodiments.
Claims
1. A method for preparing three-dimensional continuous porous carbon-supported lamellar iron-based sulfide, characterized in that The following steps are involved: 1) Add N-containing porous carbon to deionized water, add Fe salt after ultrasonic homogenization, stir vigorously to make Fe ions fully dispersed in the solution, then transfer the mixture to a high-pressure reactor, heat the high-pressure reactor in a sealed state to obtain porous carbon-loaded FeOOH, recorded as NCF; 2) adding the NCF and thioacetamide to ethylene glycol, stirring thoroughly, transferring the reaction mixture to a high-pressure reactor, sealing the high-pressure reactor for heating reaction, washing and drying after the reaction, and preparing the three-dimensional continuous porous carbon-supported lamellar iron-based sulfide.
2. The method for preparing a three-dimensional continuous porous carbon-supported lamellar iron-based sulfide according to claim 1, characterized in that In step 1), the feed ratio of the N-containing porous carbon to the Fe salt is 2-6 mg:1 mmol, preferably 4-4.5 mg:1 mmol, and the dispersion concentration of the N-containing porous carbon in deionized water is 0.5-2 mg / mL, preferably 0.8-1 mg / mL.
3. The method for preparing a three-dimensional continuous porous carbon-supported lamellar iron-based sulfide according to claim 1, characterized in that In step 1), the reaction temperature is 85-90°C and the reaction time is 10-15h.
4. The method for preparing a three-dimensional continuous porous carbon-supported lamellar iron-based sulfide according to claim 1, characterized in that In step 2), the mass ratio of NCF to thioacetamide is 1:1-10, preferably 1:3-10, and the dispersion concentration of NCF in ethylene glycol is 0.5-2 mg / mL, preferably 1-1.25 mg / mL.
5. The method for preparing a three-dimensional continuous porous carbon-supported lamellar iron-based sulfide according to claim 1, characterized in that In step 2), the reaction temperature is 130-140°C and the reaction time is 6-10h.
6. The method for preparing a three-dimensional continuous porous carbon-supported lamellar iron-based sulfide according to claim 1, characterized in that The preparation method of the N-containing porous carbon in step 1) is: melamine and sodium citrate are mixed in a mass ratio of 0.5-2:10 and fully ground, and then calcined at 600-800°C for 1-4h under an inert atmosphere, and the calcined product is stirred in a 3-5M HCl solution for 20-30h, and then the HCl solution is removed by filtration, and washed with deionized water several times until the pH of the eluent is close to neutral, and finally filtered and dried to obtain the N-containing porous carbon.
7. The method for preparing a three-dimensional continuous porous carbon-supported lamellar iron-based sulfide according to claim 6, characterized in that The mass ratio of melamine to sodium citrate is 1-1.2:10, and the roasting temperature is 700-750°C.
8. A three-dimensional continuous porous carbon-supported lamellar iron-based sulfide prepared by the method according to any one of claims 1 to 7.
9. Use of a three-dimensional continuous porous carbon-supported lamellar iron-based sulfide as claimed in claim 8 in catalytic degradation of antibiotic-contaminated water.
10. The use according to claim 9, characterized in that The Fenton catalytic system is used for catalytic degradation. A catalyst with a final concentration of 0.08-0.1 g / L and 2-4 mM H2O2 are added to the antibiotic-contaminated water body, and the catalytic degradation reaction is carried out at a pH of 4-9.
Citation Information
Patent Citations
High-stability ordered mesoporous carbon loaded Fenton catalyst, and preparation method and application thereof
CN106853370A
Preparation method of biochar-loaded iron sulfide Fenton-like catalyst
CN110773200A
Fenton reagent capable of efficiently degrading organic pollutants in alkaline environment and application of Fenton reagent
CN110803754A
FeS2 cathode heterogeneous electro-Fenton water treatment method
CN111533223A
Coralloid Fe-based / carbon composite catalyst as well as preparation method and application thereof
CN112044437A
Cited By
Method for preparing sulfur vacancy-containing thioureite and degrading antibiotics in wastewater