Preparation method of Fenton-like photocatalyst for treating naphthalene-containing sewage
By forming and modifying the Ni2[PTCDI(CO2)(SO3)] organic compound layer on the surface of the foam nickel matrix and loading the nanocrystal CeyW1-x-yMoxS2, a cerium-modified tungsten-molybdenum sulfide photocatalyst is formed, and naphthalene in naphthalene-containing wastewater treatment is solved. The problems of low degradation rate and insufficient pH adaptability have achieved efficient and stable naphthalene removal effect.
Patent Information
- Application Number
- CN202410958252.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-17
AI Technical Summary
The prior art is difficult to effectively treat naphthalene-containing wastewater, which has low naphthalene degradation rate, insufficient pH adaptation width and repeat stability, resulting in unsatisfactory treatment effect.
By forming a Ni2[PTCDI(CO2)2] organic compound layer on the surface of the foam nickel matrix, a sulfonic acid group replacement reaction is carried out to Ni2[PTCDI(CO2)(SO3)], and the nanocrystal CeyW1-x-yMoxS2 is loaded to form a foam Nickel-based Fenton photocatalysts use cerium to modify tungsten-molybdenum sulfide to improve photoquantum yield and visible light utilization, and activate hydrogen peroxide to form oxidized radicals for naphthalene degradation.
The high degradation rate, wide pH adaptability and high repeat stability treatment for naphthalene-containing wastewater are achieved, which improves the removal rate of naphthalene and the stability of the treatment system.
Smart Images

Figure CN118904361A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts for sewage treatment, in particular to a method for preparing a Fenton-like photocatalyst for treating naphthalene-containing sewage. Background Art
[0002] With the development of petroleum, coal chemical, pharmaceutical and dye industries, the problem of industrial wastewater containing aromatic hydrocarbons is becoming more and more serious. The polycyclic aromatic hydrocarbons organic pollutants in industrial wastewater containing aromatic hydrocarbons have high chemical stability, and are difficult to self-degrade and easy to enrich. Naphthalene is composed of two benzene rings sharing two adjacent carbon atoms. It is the most common representative substance of polycyclic aromatic hydrocarbons and the primary organic pollutant controlled by environmental protection departments of various countries. It is difficult to achieve the ideal treatment effect of naphthalene-containing wastewater by using conventional wastewater treatment processes such as physical adsorption, biodegradation, and ozone oxidation, which is mainly manifested in the low naphthalene degradation rate, pH adaptation width and repeated stability.
[0003] Heterogeneous visible light Fenton-like treatment is a technology that combines the photoelectric effect and Fenton-like reaction under heterogeneous conditions. Its principle is to use multi-valent metals and hydrogen peroxide in a chain reaction under light conditions to obtain hydroxyl radicals with oxidizing ability, which can effectively degrade organic pollutants.
[0004] Therefore, developing a Fenton-like photocatalyst with high naphthalene degradation rate, wide pH adaptability and good repeated stability will surely become an ideal way to break through the technical bottleneck of naphthalene-containing wastewater treatment. Summary of the invention
[0005] In order to overcome the shortcomings of the prior art, the present invention provides a method for preparing a Fenton-like photocatalyst for treating naphthalene-containing wastewater. The photocatalyst material prepared by the method has a high degradation rate, wide pH adaptability and high repeated stability for the treatment of naphthalene-containing wastewater.
[0006] The technical solution adopted by the present invention to solve its technical problem is:
[0007] The present invention provides a method for preparing a Fenton-like photocatalyst for treating naphthalene-containing wastewater, comprising the following steps performed in sequence:
[0008] Step [1] forming a Ni2[PTCDI(CO2)2] organic compound layer on the surface of the nickel foam substrate;
[0009] Step [2] converting the Ni2[PTCDI(CO2)2] into Ni2[PTCDI(CO2)(SO3)] by sulfonic acid substitution reaction;
[0010] Step [3] Loading nanocrystalline Ce on the Ni2[PTCDI(CO2)(SO3)] organic compound layer y W1-x-y Mo x S2(0 <x≤0.4,0<y≤0.3))。
[0011] Preferably, the step [1] specifically includes the following operations:
[0012] a1. Add acetanilide, ethyl carbamate, phthalic acid hydrazide and nickel chloride to deionized water and mix well to form a reaction solution;
[0013] a2. The nickel foam sample was immersed in the reaction solution and reacted at 60-90 ℃ for 20-26 hours to obtain a nickel foam having Ni2[PTCDI(CO2)2] formed on the surface, referred to as intermediate A;
[0014] Preferably, the concentration of acetanilide in the reaction solution in step a1 is 145 g / L-210 g / L, the concentration of ethyl carbamate is 110 g / L-180 g / L, the concentration of phthalhydrazide is 60 g / L-90 g / L, and the concentration of nickel chloride is 30 g / L-50 g / L.
[0015] Preferably, in step a2, the weight of the nickel foam immersed in each liter of the reaction solution is 320-370 g.
[0016] Preferably, the specific operations of step [2] are:
[0017] b1. Add 4-methylbenzenesulfonic acid, 3-aminopropanesulfonic acid and 1,2,3,4-tetrahydroquinoline to deionized water and mix well to form a replacement solution;
[0018] b2. The intermediate A is immersed in the replacement solution and reacted at 70-100 ℃ for 16-24 hours to obtain a nickel foam having a Ni2[PTCDI(CO2)(SO3)] organic compound layer formed on the surface, referred to as intermediate B;
[0019] Preferably, in the replacement solution in step b1, the concentration of 4-methylbenzenesulfonic acid is 60 g / L-100 g / L, the concentration of 3-aminopropanesulfonic acid is 40 g / L-70 g / L, and the concentration of 1,2,3,4-tetrahydroquinoline is 50 mL / L-80 mL / L.
[0020] Preferably, in step b2, the weight of the intermediate A immersed in each liter of the replacement liquid is 240-300 g.
[0021] Preferably, the step [3] specifically includes the following operations:
[0022] c1. Add ammonium molybdate, hexacarbonyl tungsten and carbon disulfide to diphenyl sulfide and mix them evenly to form a treatment solution; immerse the intermediate B in the treatment solution and react at 60-90° C. for 24-30 hours to obtain an intermediate C;
[0023] c2. Add cerium trichloride, dimethyl sulfate and diethyl oxalate to tetrahydrofuran and mix them evenly to form an organic modification solution; immerse the intermediate C in the organic modification solution and use it as a cathode, stainless steel as an anode, and electrodeposit for 30-40 minutes at room temperature with a constant voltage of 2.0 to 2.4 V to finally obtain the Fenton-like photocatalyst.
[0024] Preferably, the concentration of ammonium molybdate in the treatment solution in step c1 is 120g / L-150g / L, the concentration of tungsten hexacarbonyl is 210g / L-240g / L, and the concentration of carbon disulfide is 120mL / L-160mL / L; the weight of the intermediate B immersed in each liter of the treatment solution is 50-80g.
[0025] Preferably, the cerium trichloride concentration of the organic modification solution in step c2 is 50g / L-80g / L, the dimethyl sulfate concentration is 20mL / L-40mL / L, and the diethyl oxalate concentration is 10mL / L-30mL / L; the weight of the intermediate C immersed in each liter of the organic modification solution is 200-230g.
[0026] The positive effects of the present invention are as follows: the Fenton-like photocatalyst (foamed nickel-based Ni2[PTCDI(CO2)(SO3)] organic matter loaded Ce) prepared by the method of the present invention y W 1-x-y Mo x S2), its structural characteristics are: Ni2[PTCDI(CO2)(SO3)] organic matter is an organic compound formed by perylenetetracarboxylic acid diamide PTCDI(CO2)(SO3) with carboxyl and sulfonic acid groups replacing the imide site and nickel ions, wherein the perylenetetracarboxylic acid diamide PTCDI(CO2)(SO3) replaced by carboxyl and sulfonic acid groups is composed of five benzene rings fused together, and has a conjugated system with the characteristics of molecular coplanarity; Ce y W 1-x-y Mo x S2 is a cerium-doped hexagonal tungsten-molybdenum sulfide. y W 1-x- y Mo xS2 is a nanocrystal formed on nickel foam-based Ni2[PTCDI(CO2)(SO3)] organic matter. Tungsten-molybdenum sulfide can form an electron depletion region and an internal electric field in the interface region after being modified with cerium. Based on the above structural characteristics, the conjugated system characteristics of the molecular coplanar structure of Ni2[PTCDI(CO2)(SO3)] organic matter can make the catalytic material have a wide absorption spectrum and electron-rich characteristics; carboxyl and sulfonic acid groups replace the imide sites of perylenetetracarboxamide to effectively avoid the recombination of photogenerated carriers and improve the photocatalytic rate; the photoquantum yield and visible light utilization rate of tungsten-molybdenum sulfide modified with cerium are significantly improved, effectively avoiding the recombination of electrons and holes; under visible light irradiation, the nickel foam-based Ni2[PTCDI(CO2)(SO3)] organic matter loaded with Ce y W 1-x-y Mo x The multivalent nickel and cerium of the S2-type Fenton photocatalytic material can activate hydrogen peroxide to obtain hydroxyl radicals and superoxide radicals with strong oxidizing ability, resulting in a heterogeneous visible light-type Fenton chain reaction. Through the synergistic effect of photocatalysis and nickel and cerium ions on hydrogen peroxide, the degradation and mineralization of naphthalene in naphthalene-containing wastewater is achieved. The Fenton-type photocatalyst prepared according to the present invention has a high naphthalene degradation rate, wide pH adaptability and high repetitive stability for heterogeneous visible light-type Fenton treatment of naphthalene-containing wastewater. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic diagram of the preparation process of the Fenton-like photocatalyst of the present invention;
[0028] Figure 2 It is a schematic diagram of the structure of Ni2[PTCDI(CO2)2] of the present invention;
[0029] Figure 3 is a schematic diagram of the structure of the Ni2[PTCDI(CO2)(SO3)] organic compound of the present invention;
[0030] Figure 4a It is a comparison of the residual naphthalene percentages of Example 1, Comparative Example 1 and Comparative Example 2 of the present invention under a simulated environment of pH 4;
[0031] Figure 4b The figure is a comparison of the residual naphthalene percentages of Example 1, Comparative Example 1 and Comparative Example 2 under a simulated environment of pH 7;
[0032] Figure 4c The figure is a comparison of the residual naphthalene percentages of Example 1, Comparative Example 1 and Comparative Example 2 of the present invention under a simulated environment of pH 10;
[0033] Figure 5a It is a relationship diagram between the number of treatments and the naphthalene degradation rate of Example 1, Comparative Example 1 and Comparative Example 2 of the present invention under a simulated environment of pH 4;
[0034] Figure 5b It is a relationship diagram between the number of treatments and the naphthalene degradation rate of Example 1, Comparative Example 1 and Comparative Example 2 of the present invention under a simulated environment of pH 7;
[0035] Figure 5c It is a relationship diagram between the number of treatments and the naphthalene degradation rate of Example 1, Comparative Example 1 and Comparative Example 2 of the present invention under a simulated environment of pH 10. DETAILED DESCRIPTION
[0036] Reference Figure 1 The present invention provides a method for preparing a Fenton-like photocatalyst for treating naphthalene-containing wastewater, comprising the following steps performed in sequence:
[0037] Step [1] forms a Ni2[PTCDI(CO2)2] organic compound layer on the surface of the nickel foam substrate, specifically comprising the following operations:
[0038] a1. Add acetanilide, ethyl carbamate, phthalic acid hydrazide and nickel chloride to deionized water and mix well to form an acetanilide concentration of 145g / L-210g / L, ethyl carbamate concentration of 110g / L-180g / L, phthalic acid hydrazide concentration of 60g / L-90g / L, nickel chloride concentration of 30g / L-50g / L of the reaction solution;
[0039] a2. Immerse the nickel foam sample in the reaction solution (the weight of the nickel foam immersed in each liter of the reaction solution is 320-370g), react at 60-90°C for 20-26 hours, and obtain a nickel foam with Ni2[PTCDI(CO2)2] formed on the surface, which is recorded as intermediate A; wherein the structure of the Ni2[PTCDI(CO2)2] is as follows Figure 2 shown.
[0040] Step [2] converts the Ni2[PTCDI(CO2)2] into Ni2[PTCDI(CO2)(SO3)] by sulfonic acid substitution reaction, and the specific operation is as follows:
[0041] b1. Add 4-methylbenzenesulfonic acid, 3-aminopropanesulfonic acid and 1,2,3,4-tetrahydroquinoline to deionized water and mix well to form a 4-methylbenzenesulfonic acid concentration of 60 g / L-100 g / L, a 3-aminopropanesulfonic acid concentration of 40 g / L-70 g / L, and a 1,2,3,4-tetrahydroquinoline concentration of 50 mL / L-80 mL / L of the replacement solution;
[0042] b2. Immerse intermediate A in the replacement liquid (the weight of intermediate A immersed in each liter of the replacement liquid is 240 - 300 g), react at 70 - 100 °C for 16 - 24 hours to obtain nickel foam with an Ni2[PTCDI(CO2)(SO3)] organic compound layer formed on its surface, denoted as intermediate B; wherein, the structure of the Ni2[PTCDI(CO2)(SO3)] is as Figure 3 shown.
[0043] Step [3] Load nanocrystalline Ce y W 1-x-y Mo x S2 (0 < x ≤ 0.4, 0 < y ≤ 0.3)) on the Ni2[PTCDI(CO2)(SO3)] organic compound layer, specifically including the following operations:
[0044] c1. Add ammonium molybdate, tungsten hexacarbonyl, and carbon disulfide to diphenyl sulfide, mix evenly to form a treatment liquid with an ammonium molybdate concentration of 120 g / L - 150 g / L, a tungsten hexacarbonyl concentration of 210 g / L - 240 g / L, and a carbon disulfide concentration of 120 mL / L - 160 mL / L; immerse intermediate B in the treatment liquid (the weight of intermediate B immersed in each liter of the treatment liquid is 50 - 80 g), react at 60 - 90 °C for 24 - 30 hours to obtain intermediate C;
[0045] c2. Add cerium trichloride, dimethyl sulfate, and diethyl oxalate to tetrahydrofuran, mix evenly to form an organic modification liquid with a cerium trichloride concentration of 50 g / L - 80 g / L, a dimethyl sulfate concentration of 20 mL / L - 40 mL / L, and a diethyl oxalate concentration of 10 mL / L - 30 mL / L; immerse intermediate C in the organic modification liquid and use it as the cathode (the weight of intermediate C immersed in each liter of the organic modification liquid is 200 - 230 g), use stainless steel as the anode, at room temperature, use 2.0 - 2.4 V as the constant voltage for electrodeposition voltage, and electrodeposit for 30 - 40 minutes to finally obtain the Fenton-like photocatalyst (nickel foam-based Ni2[PTCDI(CO2)(SO3)] organic matter loaded with Ce y W 1-x-y Mo x S2).
[0046] The following is an example of the preferred embodiment of the present invention.
[0047] Example 1
[0048] The preferred embodiment 1 of the present invention provides a preparation method of a Fenton-like photocatalyst for treating naphthalene-containing sewage, including the following steps carried out in sequence:
[0049] Step [1] Form an Ni2[PTCDI(CO2)2] organic compound layer on the surface of the nickel foam substrate, which specifically includes the following operations:
[0050] a1. Add acetanilide, ethyl carbamate, phthalhydrazide, and nickel chloride to deionized water and mix evenly to form a reaction solution with an acetanilide concentration of 160 g / L, an ethyl carbamate concentration of 170 g / L, a phthalhydrazide concentration of 80 g / L, and a nickel chloride concentration of 40 g / L;
[0051] a2. Immerse the nickel foam sample in the reaction solution (the weight of the nickel foam immersed in each liter of the reaction solution is 360 g), and react at 80 °C for 26 hours to obtain nickel foam with Ni2[PTCDI(CO2)2] formed on its surface, denoted as intermediate A.
[0052] Step [2] Convert the Ni2[PTCDI(CO2)2] to Ni2[PTCDI(CO2)(SO3)] through a sulfonic acid group substitution reaction. The specific operation is as follows:
[0053] b1. Add 4-methylbenzenesulfonic acid, 3-aminopropanesulfonic acid, and 1,2,3,4-tetrahydroquinoline to deionized water and mix evenly to form a substitution solution with a 4-methylbenzenesulfonic acid concentration of 90 g / L, a 3-aminopropanesulfonic acid concentration of 65 g / L, and a 1,2,3,4-tetrahydroquinoline concentration of 70 mL / L;
[0054] b2. Immerse intermediate A in the substitution solution (the weight of intermediate A immersed in each liter of the substitution solution is 290 g), and react at 90 °C for 20 hours to obtain nickel foam with an Ni2[PTCDI(CO2)(SO3)] organic compound layer formed on its surface, denoted as intermediate B.
[0055] Step [3] Load nanocrystalline Ce y W 1-x-y Mo x S2 (0 < x ≤ 0.4, 0 < y ≤ 0.3)) on the Ni2[PTCDI(CO2)(SO3)] organic compound layer, which specifically includes the following operations:
[0056] c1. Add ammonium molybdate, tungsten hexacarbonyl, and carbon disulfide to diphenyl sulfide and mix evenly to form a treatment solution with an ammonium molybdate concentration of 145 g / L, a tungsten hexacarbonyl concentration of 230 g / L, and a carbon disulfide concentration of 150 mL / L; Immerse intermediate B in the treatment solution (the weight of intermediate B immersed in each liter of the treatment solution is 70 g), and react at 80 °C for 28 hours to obtain intermediate C;
[0057] c2. Add cerium trichloride, dimethyl sulfate and diethyl oxalate to tetrahydrofuran and mix them evenly to form an organic modification solution with a cerium trichloride concentration of 70 g / L, a dimethyl sulfate concentration of 40 mL / L and a diethyl oxalate concentration of 30 mL / L; immerse the intermediate C in the organic modification solution and use it as a cathode (the weight of the intermediate C immersed in each liter of the organic modification solution is 220 g), stainless steel is used as an anode, and at room temperature, a constant voltage of 2.2 V is used as the electrodeposition voltage for 35 minutes to finally obtain the Fenton-like photocatalyst, which is recorded as Example 1.
[0058] Comparative Example 1
[0059] This comparative example 1 provides a foam nickel-based Ni2[PTCDI(CO2)(SO3)] organic matter loaded W 1-x Mo x The preparation method of S2 material comprises the following steps performed in sequence:
[0060] Step [1] forms a Ni2[PTCDI(CO2)2] organic compound layer on the surface of the nickel foam substrate, specifically comprising the following operations:
[0061] a1. Add acetanilide, ethyl carbamate, phthalic acid hydrazide and nickel chloride to deionized water and mix well to form an acetanilide concentration of 150 g / L, ethyl carbamate concentration of 130 g / L, phthalic acid hydrazide concentration of 70 g / L, nickel chloride concentration of 40 g / L of the reaction solution;
[0062] a2. The nickel foam sample was immersed in the reaction solution (the weight of the nickel foam immersed in each liter of the reaction solution was 340 g), and reacted at 70°C for 24 hours to obtain a nickel foam with Ni2[PTCDI(CO2)2] formed on the surface, which was recorded as intermediate A.
[0063] Step [2] converts the Ni2[PTCDI(CO2)2] into Ni2[PTCDI(CO2)(SO3)] by sulfonic acid substitution reaction, and the specific operation is as follows:
[0064] b1. Add 4-methylbenzenesulfonic acid, 3-aminopropanesulfonic acid, and 1,2,3,4-tetrahydroquinoline to deionized water and mix well to form a 4-methylbenzenesulfonic acid concentration of 70 g / L, a 3-aminopropanesulfonic acid concentration of 50 g / L, and a 1,2,3,4-tetrahydroquinoline concentration of 60 mL / L of the replacement solution;
[0065] b2. Immerse intermediate A in the replacement solution (the weight of intermediate A immersed in each liter of the replacement solution is 250 g), react at 80°C for 18 hours, and obtain a nickel foam with a Ni2[PTCDI(CO2)(SO3)] organic compound layer formed on the surface, which is recorded as intermediate B.
[0066] Step [3] Load W on the Ni2[PTCDI(CO2)(SO3)] organic compound layer 1-a Mo a S2 (0 < a ≤ 0.5), specifically including the following operations:
[0067] Add ammonium molybdate, tungsten hexacarbonyl, and carbon disulfide to diphenyl sulfide, and mix evenly to form a treatment solution with an ammonium molybdate concentration of 130 g / L, a tungsten hexacarbonyl concentration of 220 g / L, and a carbon disulfide concentration of 130 mL / L; Immerse intermediate B in the treatment solution (the weight of intermediate B immersed in each liter of the treatment solution is 60 g), and react at 80 °C for 26 hours to obtain the foamed nickel-based Ni2[PTCDI(CO2)(SO3)] organic matter loaded with W 1-x Mo x S2 material, denoted as Comparative Example 1.
[0068] Comparative Example 2
[0069] This Comparative Example 2 provides a preparation method of a foamed nickel-based Ni2[PTCDI(CO2)(SO3)] organic matter material, including the following steps carried out in sequence:
[0070] Step [1] Form a Ni2[PTCDI(CO2)2] organic compound layer on the surface of the foamed nickel substrate, specifically including the following operations:
[0071] a1. Add acetanilide, ethyl carbamate, phthalhydrazide, and nickel chloride to deionized water, and mix evenly to form a reaction solution with an acetanilide concentration of 200 g / L, an ethyl carbamate concentration of 170 g / L, a phthalhydrazide concentration of 80 g / L, and a nickel chloride concentration of 35 g / L;
[0072] a2. Immerse the foamed nickel sample in the reaction solution (the weight of the foamed nickel immersed in each liter of the reaction solution is 360 g), and react at 80 °C for 24 hours to obtain the foamed nickel with Ni2[PTCDI(CO2)2] formed on the surface, denoted as intermediate A.
[0073] Step [2] Convert the Ni2[PTCDI(CO2)2] to Ni2[PTCDI(CO2)(SO3)] through a sulfonic acid group substitution reaction, and the specific operation is:
[0074] b1. Add 4-methylbenzenesulfonic acid, 3-aminopropanesulfonic acid, and 1,2,3,4-tetrahydroquinoline to deionized water, and mix evenly to form a substitution solution with a 4-methylbenzenesulfonic acid concentration of 90 g / L, a 3-aminopropanesulfonic acid concentration of 50 g / L, and a 1,2,3,4-tetrahydroquinoline concentration of 60 mL / L;
[0075] b2. Immerse the intermediate A in the replacement liquid (the weight of the intermediate A immersed in each liter of the replacement liquid is 260g), react at 90°C for 18 hours, and obtain a foamed nickel with a Ni2[PTCDI(CO2)(SO3)] organic compound layer formed on the surface, which is the foamed nickel-based Ni2[PTCDI(CO2)(SO3)] organic material, recorded as Comparative Example 2.
[0076] In order to analyze the degradation rate, pH adaptability and repetitive stability of heterogeneous Fenton-like treatment of naphthalene-containing sewage under visible light irradiation hydrogen peroxide conditions in Example 1, Comparative Example 1 and Comparative Example 2, naphthalene was added to ethanol to form an organic preparation liquid with a naphthalene concentration of 15g / L, the organic preparation liquid was mixed with deionized water to form a simulated naphthalene-containing sewage experimental liquid with a volume ratio of 1:7 of organic preparation liquid and deionized water, and the simulated naphthalene-containing sewage experimental liquid was adjusted with sodium hydroxide and hydrochloric acid to obtain a simulated naphthalene-containing sewage experimental liquid with pH values of 4, 7 and 10, respectively. 40 grams of Example 1, Comparative Example 1 and Comparative Example 2 were immersed in 500ml of simulated naphthalene-containing sewage of corresponding pH, 300W xenon lamp was used to simulate visible light irradiation, and heterogeneous Fenton-like photocatalytic treatment was carried out under 40mL hydrogen peroxide conditions, and simulated naphthalene-containing sewage samples were taken every 20 minutes, and the residual naphthalene concentration of the simulated naphthalene-containing sewage was analyzed by high performance liquid chromatography to calculate the residual percentage and degradation rate of naphthalene.
[0077] The results of the residual naphthalene percentages of Example 1, Comparative Example 1 and Comparative Example 2 under different pH simulated environments after 200 minutes of photocatalytic treatment are as follows: Figure 4a -c. The percentage of residual naphthalene in the simulated naphthalene-containing wastewater of Example 1 at pH values of 4, 7 and 10 is no more than 15%, that is, the removal rate of naphthalene is more than 85%. The percentage of residual naphthalene in the naphthalene-containing wastewater treated by Comparative Example 1 reaches 53% at a pH value of 7, and the percentage of residual naphthalene in the naphthalene-containing wastewater treated by Comparative Example 2 reaches 69% at a pH value of 4.
[0078] Example 1, Comparative Example 1 and Comparative Example 2 were used in the corresponding simulated sewage for photocatalytic treatment for 200 minutes, and then new corresponding simulated sewage was treated, and Example 1, Comparative Example 1 and Comparative Example 2 were used in a cycle. The results of the number of treatments and the naphthalene degradation rate are shown in FIG. Figure 5a -c, after Example 1 was treated with naphthalene-containing wastewater of corresponding pH for 6 times, the naphthalene degradation rate was still able to reach 85%, showing excellent repeated stability performance of heterogeneous photo-Fenton treatment of simulated naphthalene-containing wastewater; while the naphthalene degradation rates of Comparative Examples 1 and 2 decreased significantly with the increase in the number of repeated uses.
[0079] Therefore, the Fenton-like photocatalyst prepared according to the present invention has a high naphthalene degradation rate, wide pH value adaptability and high repetitive stability for heterogeneous visible light Fenton-like treatment of naphthalene-containing wastewater.
[0080] For further detailed illustration, the following provides another three embodiments.
[0081] Embodiment 2
[0082] The preferred Embodiment 2 of the present invention provides a preparation method of a Fenton-like photocatalyst for treating naphthalene-containing sewage, comprising the following steps carried out in sequence:
[0083] Step [1] forms a Ni2[PTCDI(CO2)2] organic compound layer on the surface of a nickel foam substrate, specifically including the following operations:
[0084] a1. Add acetanilide, ethyl carbamate, phthalhydrazide, and nickel chloride to deionized water, and mix evenly to form a reaction solution with an acetanilide concentration of 145 g / L, an ethyl carbamate concentration of 110 g / L, a phthalhydrazide concentration of 90 g / L, and a nickel chloride concentration of 50 g / L;
[0085] a2. Immerse the nickel foam specimen in the reaction solution (the weight of the nickel foam immersed in each liter of the reaction solution is 320 g), and react at 60 °C for 26 hours to obtain nickel foam with Ni2[PTCDI(CO2)2] formed on the surface, denoted as Intermediate A.
[0086] Step [2] converts the Ni2[PTCDI(CO2)2] into Ni2[PTCDI(CO2)(SO3)] through a sulfonic acid group substitution reaction, and the specific operation is as follows:
[0087] b1. Add p-toluenesulfonic acid, 3-aminopropanesulfonic acid, and 1,2,3,4-tetrahydroquinoline to deionized water, and mix evenly to form a substitution solution with a p-toluenesulfonic acid concentration of 100 g / L, a 3-aminopropanesulfonic acid concentration of 40 g / L, and a 1,2,3,4-tetrahydroquinoline concentration of 50 mL / L;
[0088] b2. Immerse Intermediate A in the substitution solution (the weight of Intermediate A immersed in each liter of the substitution solution is 240 g), and react at 100 °C for 16 hours to obtain nickel foam with a Ni2[PTCDI(CO2)(SO3)] organic compound layer formed on the surface, denoted as Intermediate B.
[0089] Step [3] loads nanocrystalline Ce y W 1-x-y Mo x S2(0 < x ≤ 0.4, 0 < y ≤ 0.3)), specifically including the following operations:
[0090] c1. Add ammonium molybdate, tungsten hexacarbonyl and carbon disulfide to diphenyl sulfide and mix them evenly to form a treatment solution with an ammonium molybdate concentration of 150 g / L, a tungsten hexacarbonyl concentration of 210 g / L and a carbon disulfide concentration of 120 mL / L; immerse the intermediate B in the treatment solution (the weight of the intermediate B immersed in each liter of the treatment solution is 80 g), react at 60° C. for 30 hours to obtain an intermediate C;
[0091] c2. Add cerium trichloride, dimethyl sulfate and diethyl oxalate into tetrahydrofuran and mix them evenly to form an organic modification solution with a cerium trichloride concentration of 80 g / L, a dimethyl sulfate concentration of 40 mL / L and a diethyl oxalate concentration of 10 mL / L; immerse the intermediate C in the organic modification solution and use it as a cathode (the weight of the intermediate C immersed in each liter of the organic modification solution is 200 g), stainless steel is used as an anode, and at room temperature, a constant voltage of 2.0 V is used as the electrodeposition voltage for 40 minutes to finally obtain the Fenton-like photocatalyst.
[0092] Example 3
[0093] Preferred embodiment 3 of the present invention provides a method for preparing a Fenton-like photocatalyst for treating naphthalene-containing wastewater, comprising the following steps performed in sequence:
[0094] Step [1] forms a Ni2[PTCDI(CO2)2] organic compound layer on the surface of the nickel foam substrate, specifically comprising the following operations:
[0095] a1. The acetanilide, ethyl carbamate, phthalic acid hydrazide and nickel chloride were added to deionized water and mixed to form an acetanilide concentration of 210 g / L, ethyl carbamate concentration of 180 g / L, phthalic acid hydrazide concentration of 60 g / L, nickel chloride concentration of 30 g / L of the reaction solution;
[0096] a2. The nickel foam sample was immersed in the reaction solution (the weight of the nickel foam immersed in each liter of the reaction solution was 370 g), and reacted at 90°C for 20 hours to obtain a nickel foam with Ni2[PTCDI(CO2)2] formed on the surface, which was recorded as intermediate A.
[0097] Step [2] converts the Ni2[PTCDI(CO2)2] into Ni2[PTCDI(CO2)(SO3)] by sulfonic acid substitution reaction, and the specific operation is as follows:
[0098] b1. Add 4-methylbenzenesulfonic acid, 3-aminopropanesulfonic acid, and 1,2,3,4-tetrahydroquinoline to deionized water and mix well to form a 4-methylbenzenesulfonic acid concentration of 60 g / L, a 3-aminopropanesulfonic acid concentration of 70 g / L, and a 1,2,3,4-tetrahydroquinoline concentration of 80 mL / L of the replacement solution;
[0099] b2. Immerse the intermediate A in the replacement liquid (the weight of the intermediate A immersed in each liter of the replacement liquid is 300 g), react at 70 °C for 24 hours to obtain nickel foam with an Ni2[PTCDI(CO2)(SO3)] organic compound layer formed on the surface, denoted as intermediate B.
[0100] Step [3] Load nanocrystalline Ce on the Ni2[PTCDI(CO2)(SO3)] organic compound layer y W 1-x-y Mo x S2 (0 < x ≤ 0.4, 0 < y ≤ 0.3)), which specifically includes the following operations:
[0101] c1. Add ammonium molybdate, tungsten hexacarbonyl, and carbon disulfide to diphenyl sulfide, mix evenly to form a treatment liquid with an ammonium molybdate concentration of 120 g / L, a tungsten hexacarbonyl concentration of 240 g / L, and a carbon disulfide concentration of 160 mL / L; immerse the intermediate B in the treatment liquid (the weight of the intermediate B immersed in each liter of the treatment liquid is 50 g), react at 90 °C for 24 hours to obtain intermediate C;
[0102] c2. Add cerium trichloride, dimethyl sulfate, and diethyl oxalate to tetrahydrofuran, mix evenly to form an organic modification liquid with a cerium trichloride concentration of 50 g / L, a dimethyl sulfate concentration of 20 mL / L, and a diethyl oxalate concentration of 30 mL / L; immerse the intermediate C in the organic modification liquid and use it as the cathode (the weight of the intermediate C immersed in each liter of the organic modification liquid is 230 g), use stainless steel as the anode, at room temperature, use 2.4 V as the constant voltage for electrodeposition for 30 minutes to finally obtain the Fenton-like photocatalyst.
[0103] Example 4
[0104] The preferred embodiment 4 of the present invention provides a preparation method of a Fenton-like photocatalyst for treating naphthalene-containing sewage, which includes the following steps carried out in sequence:
[0105] Step [1] Form an Ni2[PTCDI(CO2)2] organic compound layer on the surface of the nickel foam substrate, which specifically includes the following operations:
[0106] a1. Add acetanilide, ethyl carbamate, phthalhydrazide, and nickel chloride to deionized water, mix evenly to form a reaction liquid with an acetanilide concentration of 176 g / L, an ethyl carbamate concentration of 145 g / L, a phthalhydrazide concentration of 75 g / L, and a nickel chloride concentration of 40 g / L;
[0107] a2. Immerse the nickel foam sample in the reaction solution (the weight of nickel foam immersed in each liter of the reaction solution is 345 g), react at 75 °C for 23 hours to obtain nickel foam with Ni2[PTCDI(CO2)2] formed on the surface, denoted as intermediate A.
[0108] Step [2] converts the Ni2[PTCDI(CO2)2] into Ni2[PTCDI(CO2)(SO3)] through a sulfonic acid group substitution reaction. The specific operation is as follows:
[0109] b1. Add p-toluenesulfonic acid, 3-aminopropanesulfonic acid, and 1,2,3,4-tetrahydroquinoline to deionized water and mix evenly to form a substitution solution with a p-toluenesulfonic acid concentration of 80 g / L, a 3-aminopropanesulfonic acid concentration of 55 g / L, and a 1,2,3,4-tetrahydroquinoline concentration of 65 mL / L;
[0110] b2. Immerse intermediate A in the substitution solution (the weight of intermediate A immersed in each liter of the substitution solution is 270 g), react at 85 °C for 20 hours to obtain nickel foam with an organic compound layer of Ni2[PTCDI(CO2)(SO3)] formed on the surface, denoted as intermediate B.
[0111] Step [3] loads nanocrystalline Ce y W 1-x-y Mo x S2(0 < x ≤ 0.4, 0 < y ≤ 0.3)), which specifically includes the following operations:
[0112] c1. Add ammonium molybdate, tungsten hexacarbonyl, and carbon disulfide to diphenyl sulfide and mix evenly to form a treatment solution with an ammonium molybdate concentration of 135 g / L, a tungsten hexacarbonyl concentration of 225 g / L, and a carbon disulfide concentration of 140 mL / L; Immerse intermediate B in the treatment solution (the weight of intermediate B immersed in each liter of the treatment solution is 65 g), react at 75 °C for 27 hours to obtain intermediate C;
[0113] c2. Add cerium trichloride, dimethyl sulfate, and diethyl oxalate to tetrahydrofuran and mix evenly to form an organic modification solution with a cerium trichloride concentration of 65 g / L, a dimethyl sulfate concentration of 30 mL / L, and a diethyl oxalate concentration of 20 mL / L; Immerse intermediate C in the organic modification solution and use it as the cathode (the weight of intermediate C immersed in each liter of the organic modification solution is 215 g), use stainless steel as the anode, and at room temperature, use 2.2 V as the constant voltage for electrodeposition for 35 minutes to finally obtain the Fenton-like photocatalyst.
[0114] The above are only preferred embodiments of the present invention. It should be understood that the description of the above embodiments is only used to help understand the method and core ideas of the present invention, and is not used to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, etc. made within the ideas and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing a Fenton-like photocatalyst for treating naphthalene-containing wastewater, characterized in that: It contains the following steps in order: Step [1] forming a Ni2[PTCDI(CO2)2] organic compound layer on the surface of the nickel foam substrate; Step [2] converting the Ni2[PTCDI(CO2)2] into Ni2[PTCDI(CO2)(SO3)] by sulfonic acid substitution reaction; Step [3] Loading nanocrystalline Ce on the Ni2[PTCDI(CO2)(SO3)] organic compound layer y W 1-x-y Mo x S2(0 <x≤0.4,0<y≤0.3))。 2. The method for preparing a Fenton-like photocatalyst for treating naphthalene-containing wastewater according to claim 1, characterized in that: The step [1] specifically includes the following operations: a1. Add acetanilide, ethyl carbamate, phthalic acid hydrazide and nickel chloride to deionized water and mix well to form a reaction solution; a2. The nickel foam sample is immersed in the reaction solution and reacted at 60-90°C for 20-26 hours to obtain a nickel foam having Ni2[PTCDI(CO2)2] formed on the surface, which is recorded as intermediate A.
3. The method for preparing a Fenton-like photocatalyst for treating naphthalene-containing wastewater according to claim 2, characterized in that: In the reaction solution in step a1, the concentration of acetanilide is 145 g / L-210 g / L, the concentration of ethyl carbamate is 110 g / L-180 g / L, the concentration of phthalhydrazide is 60 g / L-90 g / L, and the concentration of nickel chloride is 30 g / L-50 g / L.
4. The method for preparing a Fenton-like photocatalyst for treating naphthalene-containing wastewater according to claim 2, characterized in that: In step a2, the weight of the nickel foam immersed in each liter of the reaction solution is 320-370 g.
5. The method for preparing a Fenton-like photocatalyst for treating naphthalene-containing wastewater according to claim 1, characterized in that: The specific operations of step [2] are: b1. Add 4-methylbenzenesulfonic acid, 3-aminopropanesulfonic acid and 1,2,3,4-tetrahydroquinoline to deionized water and mix well to form a replacement solution; b2. The intermediate A is immersed in the replacement solution and reacted at 70-100°C for 16-24 hours to obtain a nickel foam having a Ni2[PTCDI(CO2)(SO3)] organic compound layer formed on the surface, which is recorded as intermediate B.
6. The method for preparing a Fenton-like photocatalyst for treating naphthalene-containing wastewater according to claim 5, characterized in that: In the replacement solution in step b1, the concentration of 4-methylbenzenesulfonic acid is 60 g / L-100 g / L, the concentration of 3-aminopropanesulfonic acid is 40 g / L-70 g / L, and the concentration of 1,2,3,4-tetrahydroquinoline is 50 mL / L-80 mL / L.
7. The method for preparing a Fenton-like photocatalyst for treating naphthalene-containing wastewater according to claim 5, characterized in that: In step b2, the weight of the intermediate A immersed in each liter of the replacement liquid is 240-300 g.
8. The method for preparing a Fenton-like photocatalyst for treating naphthalene-containing wastewater according to claim 1, characterized in that: The step [3] specifically includes the following operations: c1. Add ammonium molybdate, hexacarbonyl tungsten and carbon disulfide to diphenyl sulfide and mix them evenly to form a treatment solution; immerse the intermediate B in the treatment solution and react at 60-90° C. for 24-30 hours to obtain an intermediate C; c2. Add cerium trichloride, dimethyl sulfate and diethyl oxalate to tetrahydrofuran and mix them evenly to form an organic modification solution; immerse the intermediate C in the organic modification solution and use it as a cathode, stainless steel as an anode, and electrodeposit for 30-40 minutes at room temperature with a constant voltage of 2.0 to 2.4 V to finally obtain the Fenton-like photocatalyst.
9. The method for preparing a Fenton-like photocatalyst for treating naphthalene-containing wastewater according to claim 8, characterized in that: In step c1, the concentration of ammonium molybdate in the treatment solution is 120g / L-150g / L, the concentration of tungsten hexacarbonyl is 210g / L-240g / L, and the concentration of carbon disulfide is 120mL / L-160mL / L; the weight of the intermediate B immersed in each liter of the treatment solution is 50-80g.
10. The method for preparing a Fenton-like photocatalyst for treating naphthalene-containing wastewater according to claim 8, characterized in that: In step c2, the concentration of cerium trichloride in the organic modification solution is 50g / L-80g / L, the concentration of dimethyl sulfate is 20mL / L-40mL / L, and the concentration of diethyl oxalate is 10mL / L-30mL / L; the weight of the intermediate C immersed in each liter of the organic modification solution is 200-230g.
Citation Information
Patent Citations
Method for arranging one-dimensional organic nano materials in orientating and patterning manner
CN102050428A
Preparation method of copper-based nickel ytterbium oxysulfide supported organic compound catalytic material
CN118186487A
Copolymer of formaldehyde and method for manufacturing the same
GB1000673A
Method for producing polyimide polymer, composition for polyimide-based insulation film
JP2002012664A
Synergistic peroxide based biocidal compositions
US20100092574A1