Catalyst for producing tetrahydrofuran by one-step method as well as preparation method and application of catalyst

During the preparation process of tetrahydrofuran by CuO-ZnO/inorganic acid catalyst, the problems of excessive acidity, high solvent consumption and low selectivity were solved, and efficient preparation of tetrahydrofuran was achieved, and the conversion rate and selectivity of the anemic anhydride were significantly improved.

CN118904369APending Publication Date: 2024-11-08ZHONGKE SYNTHETIC OIL INNER MONGOLIA TECH RES INST CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411038871.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art has problems such as excessive acidity in the preparation process of tetrahydrofuran, resulting in equipment corrosion, high solvent consumption, low conversion of manic anhydride and low selectivity, especially in the one-step preparation process, which is difficult to effectively solve these problems.

Method used

Using CuO-ZnO/inorganic acid catalyst, the catalyst is prepared by combining a mixed solution of copper and zinc salt with a precipitant by adding an appropriate amount of inorganic acid. After aging, filtration, washing, drying and calcining, the catalyst is prepared and reacted in a fixed bed. The gas phase hydrogenation reaction was carried out in the utensil, and the maleic anhydride was used as a raw material to convert it into tetrahydrofuran in one-step process.

Benefits of technology

A catalyst with low acid addition and low corrosion was achieved, with a conversion rate of 100% of the maleic anhydride and a selectivity of tetrahydrofuran reaching more than 98%, which significantly improved the preparation efficiency and product purity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004971845280000071
    Figure BDA0004971845280000071
Patent Text Reader

Abstract

The invention provides a catalyst for producing tetrahydrofuran by a one-step method as well as a preparation method and application of the catalyst. The catalyst is CuO-ZnO / inorganic acid, wherein the inorganic acid is phosphoric acid, phosphotungstic acid, phosphomolybdic acid, silicotungstic acid, ammonium metatungstate and the like. The catalyst has double functions of hydrogenation and dehydration. Under the catalysis of the catalyst, maleic anhydride is hydrogenated to prepare tetrahydrofuran, and the catalyst has the advantages of complete maleic anhydride conversion rate, high tetrahydrofuran selectivity, simple reaction process and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of chemical industry, and in particular to a catalyst for preparing tetrahydrofuran in one step, and a preparation method and application thereof. Background Art

[0002] Tetrahydrofuran is a completely hydrogenated product of the aromatic compound furan. It is generally a colorless, water-miscible, and low-viscosity organic liquid at room temperature. Tetrahydrofuran is an important organic synthetic raw material and a solvent with excellent performance. It is mainly used to synthesize polytetrahydrofuran, or as a reaction raw material or solvent for adhesives, inks, resins, chemicals, pharmaceuticals, extractants, etc. It is widely used in the fields of chemical industry, medicine, textiles, laboratories, etc. The mainstream production method of tetrahydrofuran in modern industry is the dehydration and cyclization method of 1,4-butanediol (BDO), which is to dehydrate and purify high-purity BDO under certain conditions to obtain tetrahydrofuran. And 1,4-butanediol can be divided into the Reppe method and the maleic anhydride esterification hydrogenation method according to the preparation method. The Reppe process includes three steps: (1) acetylene and formaldehyde are catalytically produced into 1,4-butynediol; (2) 1,4-butynediol is catalytically hydrogenated to produce 1,4-butenediol; (3) 1,4-butenediol is hydrogenated to produce 1,4-butanediol. The maleic anhydride esterification and hydrogenation process includes: (1) maleic anhydride is esterified to obtain dimethyl maleate; (2) dimethyl maleate is hydrogenated to produce 1,4-butanediol.

[0003] Patent CN108148020A discloses a method for preparing tetrahydrofuran by dehydrating 1,4-butanediol with concentrated sulfuric acid. The method uses concentrated sulfuric acid and 13X molecular sieve catalyst, has the advantages of low cost and reduced polycarbon compounds and high molecular polymer products, and can obtain a tetrahydrofuran product with a tar content of less than 5%. However, the concentrated sulfuric acid is too acidic and will cause equipment corrosion.

[0004] Patent CN1743068A discloses a method for preparing tetrahydrofuran by hydrogenating dimethyl maleate, which uses a Cu-B supported catalyst and has the advantage of high conversion rate to obtain tetrahydrofuran, but requires esterification of maleic anhydride, which increases the consumption of alcohols.

[0005] Patent CN101168535A discloses the production of tetrahydrofuran in one step by gas phase hydrogenation of maleic anhydride on Cu-Zn-Ti-Ce with n-butanol as solvent. The Cu-Zn-Ti-Ce catalyst has the advantages of high maleic anhydride conversion rate and hydrogen saving, and can produce tetrahydrofuran, hydrogen, butyl butyrate, and n-butyraldehyde, but it needs to consume solvents, and the selectivity of tetrahydrofuran is not high.

[0006] Patent CN102617518A discloses a bifunctional catalyst with copper zinc as a hydrogenation component and a solid acid as a dehydration component. Since the solid acid is weak in acidity, a higher mass percentage is required to achieve the function of BDO dehydration, which will also affect the activity of the hydrogenation component.

[0007] In summary, the prior art methods for preparing BDO from maleic anhydride and further preparing tetrahydrofuran have many deficiencies. Therefore, the present invention provides a catalyst for preparing tetrahydrofuran in one step, and its preparation method and application. Summary of the invention

[0008] The purpose of the present invention is to provide a catalyst for preparing tetrahydrofuran from maleic anhydride in a one-step process, and a preparation method and application thereof. The catalyst of the present invention has the characteristics of low acid addition amount and low corrosiveness, and has a significant effect when applied to the reaction of converting maleic anhydride into tetrahydrofuran by one-step hydrogenation with maleic anhydride as a raw material. Specifically, the maleic anhydride conversion rate can reach 100%, and the tetrahydrofuran selectivity can reach more than 98%.

[0009] On the one hand, the present invention provides a catalyst, which includes: in terms of mass percentage, 20-60 parts of CuO, 30-55 parts of ZnO, and 1-40 parts of an inorganic acid, wherein the inorganic acid is one or a mixture of two of phosphoric acid, phosphotungstic acid, phosphomolybdic acid, silicotungstic acid, and ammonium metatungstate, preferably phosphoric acid and phosphotungstic acid, and more preferably phosphotungstic acid.

[0010] In some embodiments, the catalyst is used for catalyzing maleic anhydride to prepare tetrahydrofuran in a one-step process.

[0011] In some embodiments, the catalyst comprises: by mass percentage, 40-55 parts of CuO, 40-53 parts of ZnO, and 1-10 parts of inorganic acid; preferably, the catalyst comprises: by mass percentage, 45-50 parts of CuO, 45-50 parts of ZnO, and 1-5 parts of inorganic acid; more preferably, the catalyst comprises: by mass percentage, 48 parts of CuO, 48 parts of ZnO, and 3 parts of inorganic acid.

[0012] In another aspect, the present invention provides a method for preparing a catalyst, comprising the following steps:

[0013] (1) preparing a mixed solution A of copper salt and zinc salt;

[0014] (2) preparing precipitant solution B;

[0015] (3) adding the mixed solution A described in step (1) to the precipitant solution B under stirring to obtain a mixed solution C;

[0016] (4) aging, filtering, washing, drying and calcining the mixed solution C to obtain a catalyst precursor;

[0017] (5) Adding an inorganic acid solution to the catalyst precursor and drying the mixture to obtain the catalyst.

[0018] In some embodiments, the preparation method further comprises:

[0019] (6) spraying the catalyst obtained in step (5) with deionized water, rolling, crushing and screening to obtain particles of greater than or equal to 20 and less than or equal to 40 mesh, greater than 40 and less than or equal to 60 mesh, and greater than 60 and less than or equal to 80 mesh;

[0020] (7) Catalysts with mesh sizes of 20 to 40, 40 to 60, and 60 to 80 are mixed in different proportions, and graphite powder is added at 0.1% to 10% of the mass of the catalyst, and the mixture is pressed into granules of 3 to 5 mm in a granulator.

[0021] In some embodiments, the catalyst is as described above.

[0022] In some embodiments, the anions of the copper salt and the zinc salt in step (1) are selected from nitrate ions or chloride ions, preferably nitrate ions.

[0023] In some embodiments, the total concentration of copper and zinc in the mixed solution A in step (1) is 0.1-3 mol / L, preferably 0.5-2 mol / L.

[0024] In some embodiments, the mixed solution A is an aqueous solution.

[0025] In some embodiments, the molar ratio of copper to zinc is 1-3:3-1, preferably 1-2:2-1, and more preferably 1:1.

[0026] In some embodiments, the precipitant in step (2) is one or more of sodium hydroxide, sodium carbonate, sodium bicarbonate, potassium hydroxide, potassium carbonate, and potassium bicarbonate.

[0027] In some embodiments, the concentration of the precipitant solution B in step (2) is 0.5-3 mol / L, preferably 1-2 mol / L.

[0028] In some embodiments, the precipitant solution B is an aqueous solution.

[0029] In some embodiments, step (3) is performed under heating, the heating temperature is 45-85°C, preferably 60-80°C; the stirring speed is 50-400 rpm, and the stirring time is 0.5-24h.

[0030] In some preferred embodiments, the pH value of the process in step (3) is measured, and the mixing is stopped when the pH value is 7-8.

[0031] In some embodiments, the aging conditions of step (4) are: temperature 45-90°C, time 0.5-24h; the drying conditions are: temperature 60-120°C, time 4-48h; the calcination conditions are: temperature 400-450°C, time 4-12h.

[0032] In some embodiments, the mass fraction of the inorganic acid solution in step (5) is 0.1%-10%, preferably 1%-5%.

[0033] In some embodiments, the inorganic acid solution in step (5) is an aqueous solution.

[0034] In some embodiments, in step (7), the catalysts with mesh sizes of 20 to 40 mesh, 40 to 60 mesh, and 60 to 80 mesh are mixed in a ratio of 5-25%: 60-85%: 5-20%. Preferably, the ratio is 10-20%: 65-80%: 5-15%.

[0035] In some embodiments, 1% to 5% of the mass of the catalyst is added with graphite powder in step (7).

[0036] In yet another aspect, the present invention provides a catalyst prepared by the preparation method.

[0037] In yet another aspect, the present invention provides a method for preparing tetrahydrofuran, comprising:

[0038] (1) vaporizing maleic anhydride and then mixing it with hydrogen to form a gaseous reaction mixture;

[0039] (2) passing the gaseous reaction mixture obtained in step (1) into a reactor pre-loaded with the catalyst for gas-phase hydrogenation reaction to obtain a crude tetrahydrofuran product.

[0040] In some embodiments, the reaction conditions of step (2) are as follows: the temperature is 180-260°C, preferably 200-250°C; the reaction pressure is 1-8Mpa, preferably 2-6Mpa, and the liquid weight space velocity of the raw material maleic anhydride is 0.01-0.55h -1 , preferably 0.02 to 0.1 h -1 .

[0041] In some embodiments, the method is used to catalyze maleic anhydride to prepare tetrahydrofuran in a one-step process.

[0042] Beneficial effects: The present invention provides a catalyst for preparing tetrahydrofuran from maleic anhydride in a one-step process, and a preparation method and application thereof. The catalyst of the present invention is CuO-ZuO / inorganic acid, which has the characteristics of low acid addition amount and low corrosiveness. It has a significant effect when applied to the reaction of converting maleic anhydride into tetrahydrofuran by one-step hydrogenation with maleic anhydride as a raw material. The maleic anhydride conversion rate can reach 100%, and the tetrahydrofuran selectivity can reach more than 98%, which has a good application prospect. DETAILED DESCRIPTION

[0043] The specific embodiments of the present invention are described in detail below. The specific embodiments described here are only used to illustrate and explain the present invention, but are not used to limit the present invention.

[0044] The present invention is further described below by way of examples, but the present invention is not limited thereto.

[0045] Example

[0046] Unless otherwise specified, the reagents, materials and devices involved in the following examples are all commercially available in the art; the conventional operations involved in the following examples can be found in patents, patent applications and publications disclosed in the art (for example, He Yongde, ed., "Modern Coal Chemical Technology Handbook", Chemical Industry Press, 2003, but not limited thereto).

[0047] Example 1

[0048] First, prepare 0.5 mol / L copper nitrate and zinc nitrate mixed solution (Cu / Zn molar ratio 1:1), and then prepare 1 mol / L sodium carbonate solution as a precipitant, add the copper nitrate and zinc nitrate mixed solution dropwise into the sodium carbonate solution in a 60°C water bath, stir, stop dropping when the pH value is 7-8, age for 12 hours, filter, wash, dry at 110°C for 6 hours, roast at 400°C for 4 hours, add 0.5% mass fraction of phosphoric acid for impregnation (the acid content is 3% of the total mass of the catalyst), and obtain CuO-ZnO / phosphoric acid catalyst after drying. (The content ratio of each component is 48 / 48 / 3). The dried catalyst is sprayed with deionized water and rolled, and crushed and sieved to obtain particles of greater than or equal to 20 to less than or equal to 40 mesh, greater than 40 to less than or equal to 60 mesh, and greater than 60 to less than or equal to 80 mesh. The catalysts of greater than or equal to 20 to less than or equal to 40 mesh, greater than 40 to less than or equal to 60 mesh, and greater than 60 to less than or equal to 80 mesh are mixed at mass fractions of 20%, 75%, and 5%, and then 2% of graphite powder is added and pressed into 3mm catalyst particles.

[0049] The CuO-ZnO / phosphoric acid catalyst prepared above was loaded into a fixed bed reactor, and maleic anhydride was used as a raw material to carry out a gas phase hydrogenation reaction; the process conditions were: temperature 220°C, pressure 3Mpa, maleic anhydride liquid weight space velocity 0.05h -1 The reaction results are shown in Table 1.

[0050] Example 2

[0051] First, prepare 1 mol / L copper nitrate and zinc nitrate mixed solution (Cu / Zn molar ratio 1:1), and then prepare 1.5 mol / L sodium carbonate solution as a precipitant, add the copper nitrate and zinc nitrate mixed solution dropwise to the sodium carbonate solution in a 70°C water bath, stir, stop dropping when the pH value is 7-8, age for 8 hours, filter, wash, dry at 110°C for 12 hours, roast at 450°C for 6 hours, add 1% mass fraction of phosphotungstic acid for impregnation (the acid content is 4% of the total mass of the catalyst), and obtain CuO-ZnO / phosphotungstic acid catalyst after drying. (The content ratio of each component is 48 / 48 / 3). The dried catalyst is sprayed with deionized water and rolled, and crushed and sieved to obtain particles of greater than or equal to 20 to less than or equal to 40 mesh, greater than 40 to less than or equal to 60 mesh, and greater than 60 to less than or equal to 80 mesh. The catalysts of greater than or equal to 20 to less than or equal to 40 mesh, greater than 40 to less than or equal to 60 mesh, and greater than 60 to less than or equal to 80 mesh are mixed at mass fractions of 15%, 75%, and 10%, and then 4% of graphite powder is added and pressed into catalyst particles of 4 mm.

[0052] The CuO-ZnO / phosphotungstic acid catalyst prepared above was loaded into a fixed bed reactor, and maleic anhydride was used as a raw material to carry out a gas phase hydrogenation reaction; the process conditions were: temperature 230°C, pressure 2.5 MPa, maleic anhydride liquid weight space velocity 0.1 h -1 The reaction results are shown in Table 1.

[0053] Example 3

[0054] First, prepare 1.5 mol / L copper nitrate and zinc nitrate mixed solution (Cu / Zn molar ratio 1:1), and then prepare 2 mol / L sodium carbonate solution as a precipitant, add the copper nitrate and zinc nitrate mixed solution dropwise to the sodium carbonate solution in an 80°C water bath, stir, stop dropping when the pH value is 7-8, age for 6 hours, filter, wash, dry at 100°C for 12 hours, roast at 450°C for 8 hours, add 3% mass fraction of phosphomolybdic acid for impregnation (the acid content is 5% of the total mass of the catalyst), and obtain CuO-ZnO / phosphomolybdic acid catalyst after drying. (The content ratio of each component is 48 / 48 / 3). The dried catalyst is sprayed with deionized water and rolled, and crushed and sieved to obtain particles of greater than or equal to 20 to less than or equal to 40 mesh, greater than 40 to less than or equal to 60 mesh, and greater than 60 to less than or equal to 80 mesh. The catalysts of greater than or equal to 20 to less than or equal to 40 mesh, greater than 40 to less than or equal to 60 mesh, and greater than 60 to less than or equal to 80 mesh are mixed at mass fractions of 10%, 80%, and 10%, and then 3% of graphite powder is added and pressed into 3mm catalyst particles.

[0055] The CuO-ZnO / phosphomolybdic acid catalyst prepared above was loaded into a fixed bed reactor, and maleic anhydride was used as a raw material to carry out a gas phase hydrogenation reaction; the process conditions were: temperature 250°C, pressure 3 MPa, maleic anhydride liquid weight space velocity 0.1 h -1 The reaction results are shown in Table 1.

[0056] Example 4

[0057] First, prepare 1 mol / L copper nitrate and zinc nitrate mixed solution (Cu / Zn molar ratio 1:1), and then prepare 1.5 mol / L sodium carbonate solution as a precipitant, add the copper nitrate and zinc nitrate mixed solution to the sodium carbonate solution in a 70°C water bath, stir, stop adding when the pH value is 7-8, age for 4 hours, filter, wash, dry at 110°C for 12 hours, roast at 450°C for 4 hours, add 5% mass fraction of silicotungstic acid for impregnation (the acid content is 6% of the total mass of the catalyst), and obtain CuO-ZnO / silicotungstic acid catalyst after drying. (The content ratio of each component is 48 / 48 / 3). The dried catalyst is sprayed with deionized water and rolled, and crushed and sieved to obtain particles of greater than or equal to 20 and less than or equal to 40 mesh, greater than 40 and less than or equal to 60 mesh, and greater than 60 and less than or equal to 80 mesh. The catalysts of greater than or equal to 20 and less than or equal to 40 mesh, greater than 40 and less than or equal to 60 mesh, and greater than 60 and less than or equal to 80 mesh are mixed at mass fractions of 20%, 65%, and 15%, and then 5% of graphite powder is added to press into catalyst particles of 5 mm.

[0058] The CuO-ZnO / silicotungstic acid catalyst prepared above was loaded into a fixed bed reactor, and maleic anhydride was used as a raw material to carry out a gas phase hydrogenation reaction; the process conditions were: temperature 240°C, pressure 1 MPa, maleic anhydride liquid weight space velocity 0.08 h -1 The reaction results are shown in Table 1.

[0059] Table 1: Comparison of reaction conversion and selectivity under different catalysts

[0060]

[0061] It should be noted that the present invention is particularly described using individual embodiments. However, without departing from the principles of the present invention, a person skilled in the art may make various improvements in form or detail to the present invention, and these improvements also fall within the scope of protection of the present invention.

Claims

1. A catalyst, comprising: In terms of mass percentage, the invention comprises 20-60 parts of CuO, 30-55 parts of ZnO, and 1-40 parts of an inorganic acid, wherein the inorganic acid is one or a mixture of two of phosphoric acid, phosphotungstic acid, phosphomolybdic acid, silicotungstic acid, and ammonium metatungstate, preferably phosphoric acid and phosphotungstic acid, and more preferably phosphotungstic acid.

2. The catalyst according to claim 1, characterized in that The catalyst comprises, by mass percentage, 40-55 parts of CuO, 40-53 parts of ZnO, and 1-10 parts of inorganic acid; preferably, the catalyst comprises, by mass percentage, 45-50 parts of CuO, 45-50 parts of ZnO, and 1-5 parts of inorganic acid; more preferably, the catalyst comprises, by mass percentage, 48 parts of CuO, 48 parts of ZnO, and 3 parts of inorganic acid.

3. A method for preparing a catalyst, comprising the following steps: (1) preparing a mixed solution A of copper salt and zinc salt; (2) preparing precipitant solution B; (3) adding the mixed solution A described in step (1) to the precipitant solution B under stirring to obtain a mixed solution C; (4) aging, filtering, washing, drying and calcining the mixed solution C to obtain a catalyst precursor; (5) Adding an inorganic acid solution to the catalyst precursor and drying the mixture to obtain the catalyst.

4. The preparation method according to claim 3, characterized in that: The preparation method further comprises: (6) spraying the catalyst obtained in step (5) with deionized water, rolling, crushing and screening to obtain particles of greater than or equal to 20 and less than or equal to 40 mesh, greater than 40 and less than or equal to 60 mesh, and greater than 60 and less than or equal to 80 mesh; (7) Catalysts with mesh sizes of 20 to 40, 40 to 60, and 60 to 80 are mixed in different proportions, and graphite powder is added at 0.1% to 10% of the mass of the catalyst, and the mixture is pressed into granules of 3 to 5 mm in a granulator.

5. The preparation method according to claim 3 or 4, characterized in that: The anions of the copper salt and the zinc salt in step (1) are selected from nitrate ions or chloride ions, preferably nitrate ions; the total concentration of copper and zinc in the mixed solution A of step (1) is 0.1-3 mol / L, preferably 0.5-2 mol / L; the molar ratio of copper to zinc is 1-3:3-1, preferably 1-2:2-1, and more preferably 1:

1.

6. The preparation method according to claim 3 or 4, characterized in that: The precipitant in step (2) is one or more of sodium hydroxide, sodium carbonate, sodium bicarbonate, potassium hydroxide, potassium carbonate, and potassium bicarbonate; the concentration of the precipitant solution B in step (2) is 0.5-3 mol / L, preferably 1-2 mol / L.

7. The preparation method according to claim 3 or 4, characterized in that: The pH value of the process in step (3) is measured, and the mixing is stopped when the pH value is 7-8.

8. The preparation method according to claim 3 or 4, characterized in that: The mass fraction of the inorganic acid solution in step (5) is 0.1%-10%, preferably 1%-5%.

9. A catalyst prepared according to the preparation method according to any one of claims 3 to 8.

10. A method for preparing tetrahydrofuran, comprising: (1) vaporizing maleic anhydride and then mixing it with hydrogen to form a gaseous reaction mixture; (2) Passing the gaseous reaction mixture obtained in step (1) into a reactor pre-loaded with the catalyst according to claim 1 or 2 or the catalyst according to claim 9 for gas-phase hydrogenation reaction to obtain a crude tetrahydrofuran product.

Citation Information

Patent Citations

  • One-step preparation method for tetrahydrofuran by gas phase hydrogenating maleic anhydride on Cu-Zn-Ti-Ge and using n-butylalcohol as solvent

    CN101168535A

  • One-step preparation method for tetrahydrofuran by employing maleic anhydride gas phase hydrogenation

    CN102617518A

  • Method for preparing tetrahydrofuran through liquid-phase dehydration of 1, 4-butanediol catalyzed by concentrated sulfuric acid

    CN108148020A

  • Copper-boron catalyst for preparing butylene oxide by hydrogenating dimethyl maleate and preparing method

    CN1743068A

  • Phosphotungstic acid modified catalyst, preparation method and application in acrolein preparation thereof

    CN101786020A