Method for recycling inactivated caprolactam hydrogenation catalyst
Through crushing and strong alkali calcination treatment combined with pseudo-thin aluminite and nickel nitrate treatment, the activity of the inactivated caprolactam hydrogenation catalyst was successfully restored, solving the problems of short catalyst life and waste of resources, and achieving cost-effective catalyst regeneration.
Patent Information
- Application Number
- CN202410954684.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, the activity of caprolactam hydrorefining catalyst is reduced due to hydration reaction and accumulation of organic matter after long-term use, the catalyst life is short, and the recycling method is limited, resulting in waste of resources and increased solid waste.
The slurry is made by pulverizing the inactivated catalyst and mixing it with a strong alkali aqueous solution. After filtration and calcining, combined with the treatment of pseudo-thin aluminite and nickel nitrate, the catalyst activity is restored through hydrogen reduction to form a regeneration catalyst.
Effectively restore catalyst activity to fresh levels, reduce usage costs, extend catalyst life, and reduce resource waste and solid waste generation.
Smart Images

Figure BDA0004948399690000031 
Figure BDA0004948399690000061 
Figure BDA0004948399690000081
Abstract
Description
Technical Field
[0001] This invention relates to a method for recovering and utilizing deactivated caprolactam hydrogenation catalyst, belonging to the fields of catalysis science and chemical engineering technology. Background Technology
[0002] Caprolactam is an important chemical raw material for the production of nylon-6 fiber and engineering plastics. Its production process involves many types of raw materials and is complex. Among them, the impurities introduced by the ammoniation and rearrangement reactions number more than 30. The hydrogenation refining process mainly involves hydrogenating unsaturated substances in the impurities that have similar properties to caprolactam, so that they can be removed in the subsequent evaporation and distillation units.
[0003] Currently, the Ni / γ-Al2O3 system is mainly used for fixed-bed hydrorefining catalysts. The main reasons for their deactivation are: (1) the catalyst is immersed in caprolactam aqueous solution for a long time, and γ-Al2O3 will slowly undergo hydration reaction, causing the catalyst body to crack and break, and then be lost; (2) organic matter accumulates in the catalyst channels, covering the active sites, causing the catalyst to deteriorate in hydrogenation performance, and then gradually lose its activity. According to statistics, the life of fixed-bed caprolactam hydrorefining catalysts is generally about 1 year. Because of its high nickel content (≥25%), if it is treated as solid waste, it will cause resource waste. Therefore, it is necessary to recycle it to reduce the amount of solid waste generated, save resources, and improve economic benefits.
[0004] No research has been reported on the recycling of catalysts for caprolactam hydrogenation refining. The industry mostly uses steam purging to extend catalyst life, but the effect is limited, generally only extending the life by 1 to 2 months. Furthermore, the steam purging process may cause problems such as catalyst pulverization and increased pressure drop. Summary of the Invention
[0005] In view of the problems existing in the prior art, the purpose of this invention is to provide a method for recovering and utilizing deactivated caprolactam hydrogenation catalyst. This method is simple, easy to operate, and can restore the catalyst activity to the level of a fresh catalyst.
[0006] The technical solution adopted in this invention is as follows:
[0007] A method for recovering and utilizing a deactivated caprolactam hydrogenation catalyst includes the following steps:
[0008] (1) Mix the crushed deactivated hydrogenation catalyst with a strong alkaline aqueous solution with a concentration of 1-5 wt% to prepare slurry A, and then continue mixing at 60-80°C for 5-8 hours;
[0009] (2) The slurry A is filtered to obtain a catalyst filter cake layer. The filter cake layer is washed with deionized water and then dried to obtain filter cake B.
[0010] (3) After calcining filter cake B in an air atmosphere of 0.2-0.4 MPa at 220-560°C for 3-12 hours, crush it to a particle size of no more than 20 micrometers to obtain powder C;
[0011] (4) Powder C is uniformly mixed with boehmite, then nitric acid aqueous solution is added and extruded into strips, and then calcined at 450-600℃ for 3-6 hours to obtain catalyst intermediate D;
[0012] (5) The catalyst intermediate D is soaked in an aqueous solution of phosphoric acid and then dried, and then calcined at 500-600°C for 3-6 hours to obtain catalyst intermediate E;
[0013] (6) Catalyst intermediate E is soaked in nickel nitrate aqueous solution, then dried and calcined at 500-600℃ for 3-6 hours to obtain catalyst intermediate F;
[0014] (7) The catalyst intermediate F is reduced with hydrogen to obtain the regenerated catalyst.
[0015] In some embodiments, in step (1), the deactivated hydrogenation catalyst is derived from a fixed-bed caprolactam hydrogenation refining process unit, the active component of the catalyst is Ni, and the support is activated alumina, such as a Ni / γ-Al2O3 catalyst.
[0016] In some embodiments, in step (1), the particle size of the pulverized deactivated hydrogenation catalyst is 60 to 80 micrometers.
[0017] In some embodiments, in step (1), the strong base is one or a combination of sodium hydroxide and potassium hydroxide. Preferably, the concentration of the aqueous solution of the strong base is 1–3 wt%.
[0018] In some embodiments, in step (1), the total solids of the slurry A are controlled at 10wt% to 30wt%.
[0019] In some embodiments, in step (1), the temperature of the strong alkaline aqueous solution is controlled within the range of 60 to 80°C.
[0020] In some implementations, the mixing in step (1) can be done in any way, as long as the materials can be mixed evenly, such as stirring.
[0021] In some embodiments, in step (2), slurry A can be filtered in a plate and frame filter press, with the pressure inside the plate and frame filter press controlled within the range of 0.2 to 0.4 MPa.
[0022] In some implementations, in step (2), the conductivity of the deionized water is not higher than 5 μs / cm.
[0023] In some embodiments, in step (2), the filter cake layer is washed with deionized water until the conductivity of the washing liquid drops below 300 μs / cm, and then dried.
[0024] In some embodiments, in step (3), the roasting is carried out in a positive pressure roasting furnace, and the pressure fluctuation range of the positive pressure roasting furnace is controlled within ±0.1MPa.
[0025] In some embodiments, the calcination process in step (3) at 220–560°C is as follows: maintaining a constant temperature of 220–240°C for 1–4 hours, preferably 2 hours; maintaining a constant temperature of 370–390°C for 1–4 hours, preferably 2 hours; maintaining a constant temperature of 440–460°C for 1–4 hours, preferably 2 hours; and maintaining a constant temperature of 540–560°C for 3–6 hours, preferably 4 hours.
[0026] In some embodiments, in step (4), the hydrazine gel solubility index is not less than 95%, and its amount is 30% to 50% of the weight of powder C.
[0027] In some embodiments, in step (4), the concentration of the nitric acid aqueous solution is 8wt% to 15wt%, preferably 10wt% to 15wt%; the amount of the nitric acid aqueous solution is 0.8 to 1.1 times the weight of powder C.
[0028] In some embodiments, the roasting time in step (4) is 3 to 6 hours.
[0029] In some embodiments, in step (5), the concentration of the phosphoric acid aqueous solution is 1wt% to 3wt%, preferably 1wt% to 2wt%; and the soaking time is 40 to 80 minutes.
[0030] In some embodiments, in step (6), the concentration of nickel nitrate in the nickel nitrate aqueous solution is determined based on the nickel content in catalyst intermediate E and the water absorption rate of catalyst intermediate E, to ensure that the nickel content in catalyst intermediate F is not less than 25%. The concentration of the nickel nitrate aqueous solution is expressed in the form of grams of nickel nitrate per gram of water, and the specific calculation formula is as follows:
[0031]
[0032] Note: In formula (1), a is the nickel content (wt%) in catalyst intermediate E; b is the water absorption rate (wt%) of catalyst intermediate E.
[0033] In some embodiments, in step (6), the catalyst intermediate E is soaked in an aqueous nickel nitrate solution for 40 to 80 minutes.
[0034] In some embodiments, the roasting time in step (6) is 3 to 6 hours.
[0035] In some embodiments, in step (7), hydrogen reduction is carried out at 450–500°C.
[0036] In some embodiments, in step (7), the regenerated catalyst is stored in deoxygenated water and its hydrogenation performance is comparable to that of the fresh catalyst.
[0037] In some embodiments, the drying step in the above method can be carried out at 100-130°C.
[0038] Beneficial effects:
[0039] This invention discovers that, since the caprolactam hydrogenation refining process is a liquid-phase hydrogenation process, there are no substances such as sulfur, arsenic, or chlorine in the raw materials that would permanently deactivate the catalyst. Furthermore, the hydrogenation process is carried out at low temperatures, without side reactions such as carbon deposition or polymerization. Therefore, the main reason for catalyst deactivation is the adsorption and covering of active components by organic matter and blockage of the support pores. This invention can fully remove the organic matter adsorbed on the surface of the active components and in the support pores by pulverizing the deactivated catalyst, washing it with a strong alkaline solution, and calcining it under positive pressure at high temperature. After reshaping and nickel replenishment, the catalyst strength and nickel content can be restored, and the catalyst activity can be restored to the level of a fresh catalyst.
[0040] In the catalyst preparation process of this invention, the process from deactivated hydrogenation catalyst to powder C can be easily obtained in conventional catalyst production plants without additional investment. The raw material cost for catalyst regeneration is only 12% to 13% of that for fresh catalyst, which can significantly reduce the cost of catalyst use.
[0041] The present invention has been described in detail above; however, the above embodiments are merely illustrative in nature and are not intended to limit the invention. Furthermore, this document is not limited to the foregoing prior art or the invention itself, or to any theory described in the following embodiments.
[0042] Unless otherwise expressly stated, numerical ranges throughout the application include any subranges therein and any numerical values incremented by the smallest subunit of a given value. Unless otherwise expressly stated, numerical values throughout the application represent approximate measures or limitations on the range of embodiments including minor deviations from a given value and having approximately the mentioned value as well as having the mentioned precise value. Except in the detailed description of the working embodiments provided at the end, all numerical values of parameters (e.g., quantities or conditions) in this application (including the appended claims) should in all cases be understood to be modified by the term “approximately,” regardless of whether “approximately” actually precedes the numerical value. “Approximately” indicates that the stated numerical value allows for slight inaccuracies (some close to precision at that value; approximately or reasonably close to the value; approximate). If the inaccuracy provided by “approximately” is not understood in this common sense in the art, then “approximately” as used herein at least indicates a variation that can be produced by common methods of measuring and using these parameters. For example, “approximately” can include variations less than or equal to 10%, less than or equal to 5%, less than or equal to 4%, less than or equal to 3%, less than or equal to 2%, less than or equal to 1%, or less than or equal to 0.5%. Attached Figure Description
[0043] Figure 1 This is a pore size distribution diagram of the regenerated catalyst prepared in Example 2.
[0044] Figure 2 The image shows the pore size distribution of the fresh caprolactam hydrogenation refining catalyst in Comparative Example 1.
[0045] Figure 3 The image shows the pore size distribution of the regenerated catalyst prepared in Comparative Example 3.
[0046] Figure 4 The image shows the pore size distribution of the regenerated catalyst prepared in Comparative Example 4.
[0047] Figure 5 The image shows the pore size distribution of the regenerated catalyst prepared in Comparative Example 5. Detailed Implementation
[0048] The present invention will be further illustrated by the following examples, but these examples do not limit the scope of the invention.
[0049] Reagents and sources
[0050] Raw material name Specification supplier Sodium hydroxide AR (Shanghai Trial) (granular), ≥96.0% Sinopharm Chemical Reagent Co., Ltd. pseudoboehmite GR (Wokai) Sinopharm Chemical Reagent Co., Ltd. Nickel nitrate AR (Shanghai test), ≥98.0% Sinopharm Chemical Reagent Co., Ltd. Nitric acid AR (Shanghai Trial), 65.0%–68.0% Sinopharm Chemical Reagent Co., Ltd. Phosphoric acid AR (Shanghai test), >85.0% Sinopharm Chemical Reagent Co., Ltd.
[0051] instrument:
[0052] Particle size was measured using a laser particle size analyzer: Shanghai Sibaiji Instrument System Co., Ltd., Laser Particle Size Analyzer Mastersizer3000;
[0053] Pore size was measured using nitrogen adsorption-desorption method: McMurray Instruments (Shanghai) Co., Ltd., pore size analyzer ASAP2460.
[0054] Example 1:
[0055] 1) Take 500g of deactivated hydrogenation catalyst from Company A's caprolactam unit, crush it to 60 micrometers, and put it into 1178.45g of 1wt% sodium hydroxide aqueous solution at 60℃. Control the temperature at 60℃, stir and mix evenly to obtain slurry A; continue stirring for 5 hours with the stirring on, and maintain the temperature at 60℃.
[0056] 2) Slurry A is pumped into a small plate and frame filter press. The pressure inside the plate and frame filter press does not exceed 0.4 MPa. The catalyst filter cake layer is obtained by pressure filtration. Deionized water (conductivity not higher than 5 μs / cm) is introduced into the plate and frame filter press to wash the filter cake layer online until the conductivity of the washing liquid drops below 300 μs / cm. The filter cake layer is then dried at 120℃ to obtain filter cake B.
[0057] 3) Place filter cake B in a positive pressure calcination furnace (pressure fluctuation range controlled within ±0.1MPa) and calcine for 10 hours under a 0.2MPa air atmosphere and specific high temperature conditions. The specific high temperature conditions are: 230℃ constant temperature for 2 hours, 380℃ constant temperature for 2 hours, 450℃ constant temperature for 2 hours, and 550℃ constant temperature for 4 hours. After calcination, crush the filter cake to below 20 micrometers to obtain powder C.
[0058] 4) Take 100g of powder C and 30g of pseudoboehmite and mix them evenly. Then add 80g of 15wt% nitric acid aqueous solution, extrude into strips, and then calcine at 500℃ for 3 hours to obtain 1.2-1.4mm clover-shaped catalyst intermediate D.
[0059] 5) The catalyst intermediate D was soaked in a 1 wt% phosphoric acid aqueous solution for 50 minutes, then dried in an oven at 100°C, and then calcined at 500°C for 4 hours to obtain the catalyst intermediate E.
[0060] 6) The water absorption rate of catalyst intermediate E was measured to be 53% and the nickel content was 23%. The concentration of nickel nitrate aqueous solution was calculated to be 0.157 g Ni(NO3)2 / g H2O according to the following formula (1); 30 g of catalyst intermediate E was soaked in nickel nitrate solution for 40 minutes, and then dried at 120°C and calcined at 500°C for 3 hours to obtain catalyst intermediate F. The nickel content in catalyst intermediate F was found to be 25.2%.
[0061]
[0062] Note: In formula (1), a is the nickel content (wt%) in catalyst intermediate E; b is the water absorption rate (wt%) of catalyst intermediate E.
[0063] 7) The catalyst intermediate F is reduced with hydrogen at 500°C and then stored in deoxygenated water to obtain the regenerated catalyst product.
[0064] Example 2:
[0065] 1) Take 500g of deactivated hydrogenation catalyst from Company B's caprolactam unit, crush it to 80 microns, and put it into 1804.12g of 3wt% potassium hydroxide aqueous solution at 80℃. Control the temperature at 80℃, stir and mix evenly to obtain slurry A; continue stirring for 5 hours with the stirring on, and maintain the temperature at 80℃.
[0066] 2) Slurry A is pumped into a small plate and frame filter press. The pressure inside the plate and frame filter press does not exceed 0.3 MPa. The catalyst filter cake layer is obtained by pressure filtration. Deionized water (conductivity not higher than 5 μs / cm) is introduced into the plate and frame filter press to wash the filter cake online until the conductivity of the washing liquid drops below 300 μs / cm. The filter cake layer is then dried at 130℃ to obtain filter cake B.
[0067] 3) Place filter cake B in a positive pressure calcination furnace (pressure fluctuation range controlled within ±0.1MPa) and calcine for 10 hours under specific high temperature conditions in an air atmosphere of 0.3MPa. The specific high temperature conditions are: constant temperature of 230℃ for 2 hours, constant temperature of 380℃ for 2 hours, constant temperature of 450℃ for 2 hours, and constant temperature of 550℃ for 4 hours. After calcination, crush the filter cake to below 20 micrometers to obtain powder C.
[0068] 4) Take 100g of powder C and mix it evenly with 30g of pseudoboehmite, then add 100g of 10wt% nitric acid aqueous solution, extrude it into strips, and then calcine it at 500℃ for 4 hours to obtain 1.2-1.4mm clover-shaped catalyst intermediate D;
[0069] 5) The catalyst intermediate D was soaked in a 2wt% phosphoric acid aqueous solution for 60 minutes, then dried in an oven at 100°C, and then calcined at 500°C for 5 hours to obtain the catalyst intermediate E.
[0070] 6) The water absorption rate of catalyst intermediate E was measured to be 51.6 wt%, and the nickel content was 20 wt%. The concentration of nickel nitrate aqueous solution was calculated to be 0.402 g Ni(NO3)2 / g H2O according to formula (1). 30 g of catalyst intermediate E was soaked in nickel nitrate solution for 40 minutes, and then dried at 120℃ and calcined at 500℃ for 4 hours to obtain catalyst intermediate F. The nickel content in catalyst intermediate F was found to be 25.1 wt%.
[0071] 7) Catalyst intermediate F is reduced with hydrogen at 480℃ and then stored in deoxygenated water to obtain the regenerated catalyst product. Its pore size distribution is analyzed by nitrogen adsorption-desorption method, as shown in the figure below. Figure 1 As shown.
[0072] Comparative Example 1:
[0073] The comparative example is a fresh caprolactam hydrogenation refining catalyst of the same type as the deactivated hydrogenation catalyst in Company A's caprolactam unit in Example 1. Its pore size distribution diagram is shown below. Figure 2 As shown.
[0074] Comparative Example 2:
[0075] The preparation process of Comparative Example 2 is the same as that of Example 1, except that in step 1), the temperature of the nickel nitrate aqueous solution and the temperature during stirring are both controlled at 30°C.
[0076] Comparative Example 3:
[0077] The preparation process of Comparative Example 3 was the same as that of Example 2, except that in step 1), the slurry A was continuously stirred for 3 hours. The pore size distribution of the prepared regenerated catalyst, as determined by nitrogen adsorption-desorption method, is shown below. Figure 3 As shown.
[0078] Comparative Example 4:
[0079] The preparation process of Comparative Example 4 was the same as that of Example 2, except that in step 3), the pressure in the positive pressure calcination furnace was atmospheric pressure. The pore size distribution of the prepared regenerated catalyst, as determined by nitrogen adsorption-desorption method, is shown below. Figure 4 As shown.
[0080] Comparative Example 5:
[0081] The preparation process of Comparative Example 5 was the same as that of Example 1, except that in step 3), the positive pressure calcination temperature conditions were changed to: 130℃ for 2 hours, 300℃ for 2 hours, 450℃ for 1 hour, and 600℃ for 4 hours. The pore size distribution of the prepared regenerated catalyst, as determined by nitrogen adsorption-desorption method, is shown below. Figure 5 As shown.
[0082] Performance testing and results analysis
[0083] from Figure 1 , Figure 2 It can be seen that the pore size distribution diagram of Example 2 is very similar to that of the fresh catalyst, indicating that after treatment by the method of this invention, the pore structure of the deactivated catalyst is basically restored to the level of the fresh catalyst; from Figure 3It can be seen that insufficient stirring time for slurry A results in excessive residue of impurities on the deactivated catalyst, which cannot be completely removed even after high-temperature calcination. The catalyst pores are not fully released, negatively impacting the hydrogenation effect. Figure 4 It can be seen that atmospheric pressure roasting cannot completely remove impurities from the catalyst channels, resulting in insufficient release of catalyst from the channels and negatively impacting the hydrogenation effect; from Figure 5 It can be seen that an unreasonable temperature control program setting will cause impurities to be released in a concentrated manner in the high-temperature section, resulting in a significant increase in the size of the catalyst pores, which is detrimental to the hydrogenation selectivity of the catalyst.
[0084] The hydrogenation performance of the regenerated catalysts prepared in Examples 1-2 and the catalysts in Comparative Examples 1-5 was tested. The caprolactam aqueous solution used in the test was taken from the inlet process feed liquid of the hydrogenation reactor of the industrial caprolactam refining unit. The test results after 72 hours of reaction are listed in Table 1.
[0085] Table 1
[0086]
[0087] The PAN value characterizes the content of reducing impurities in caprolactam aqueous solution; a lower value indicates a lower content of reducing impurities. Table 1 shows that the hydrogenation effects of Examples 1-2 are basically the same as those of Comparative Example 1, indicating that the hydrogenation performance of the catalyst samples treated according to the method of this invention is close to that of fresh catalysts. This provides an environmentally friendly and economical treatment method for the purification of deactivated hydrogenation catalysts. The hydrogenation performance of the catalysts in Comparative Examples 2-5 is significantly worse than that of the catalysts prepared in Examples 1 and 2, indicating that the parameters given in this invention, such as alkaline washing temperature, stirring time, calcination pressure, and calcination temperature, are precisely sufficient to remove organic matter adsorbed on the surface of the active component and within the pores of the support. Furthermore, the catalyst strength and nickel content can be restored through reshaping and nickel replenishment processes, restoring the catalyst activity to the level of fresh catalysts.
[0088] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.
Claims
1. A method for recycling a deactivated caprolactam hydrogenation catalyst, comprising the following steps: (1) mixing the crushed deactivated hydrogenation catalyst with a 1-5 wt% strong alkali aqueous solution to form a slurry A, and then continuously mixing at 60-80° C. for 5-8 hours; (2) Slurry A is filtered to obtain a catalyst filter cake layer, the filter cake layer is washed with deionized water and then dried to obtain filter cake B; (3) calcining the filter cake B in an air atmosphere of 0.2-0.4 MPa at 220-560° C. for 3-12 hours, and crushing the filter cake B into particles no larger than 20 μm to obtain powder C; (4) Powder C and pseudo-boehmite are uniformly mixed, and then nitric acid aqueous solution is added to extrude into strips, and then calcined at 450-600° C. for 3-6 hours to obtain catalyst intermediate D; (5) The catalyst intermediate D is immersed in a phosphoric acid aqueous solution and then dried, and then calcined at 500-600° C. for 3-6 hours to obtain a catalyst intermediate E; (6) immersing the catalyst intermediate E in a nickel nitrate aqueous solution, drying it, and calcining it at 500-600° C. for 3-6 hours to obtain a catalyst intermediate F; (7) The catalyst intermediate F is reduced by hydrogen to obtain a regenerated catalyst.
2. The method for recycling a deactivated caprolactam hydrogenation catalyst according to claim 1, characterized in that: In step (1): The deactivated hydrogenation catalyst is derived from a fixed-bed caprolactam hydrogenation refining process device, the catalyst active component is Ni, the carrier is activated alumina, preferably a Ni / γ-Al2O3 catalyst; and / or The particle size of the crushed deactivated hydrogenation catalyst is 60 to 80 microns; and / or The strong base is sodium hydroxide or potassium hydroxide or a combination of the two; preferably, the concentration of the strong base aqueous solution is 1 to 3 wt%; and / or The total solid content of the slurry A is controlled at 10 wt% to 30 wt%; and / or The temperature of the strong alkali aqueous solution is controlled in the range of 60-80°C.
3. The method for recycling a deactivated caprolactam hydrogenation catalyst according to claim 1, characterized in that: In step (2): The slurry A is filtered in a plate and frame filter, and the pressure in the plate and frame filter is controlled within the range of 0.2 to 0.4 MPa; and / or The electrical conductivity of the deionized water is not higher than 5 μs / cm; and / or The filter cake layer was washed with deionized water until the conductivity of the washing liquid dropped below 300 μs / cm and then dried.
4. The method for recycling a deactivated caprolactam hydrogenation catalyst according to claim 1, characterized in that: In step (3): The roasting is carried out in a positive pressure roasting furnace, and the pressure fluctuation range of the positive pressure roasting furnace is controlled within ±0.1MPa; and / or The calcination procedure at 220-560°C is as follows: maintain a constant temperature of 220-240°C for 1-4 hours, preferably 2 hours; maintain a constant temperature of 370-390°C for 1-4 hours, preferably 2 hours; maintain a constant temperature of 440-460°C for 1-4 hours, preferably 2 hours; maintain a constant temperature of 540-560°C for 3-6 hours, preferably 4 hours.
5. The method for recycling a deactivated caprolactam hydrogenation catalyst according to claim 1, characterized in that: In step (4): The peptization index of the pseudo-boehmite is not less than 95%, and the amount thereof is 30% to 50% of the weight of the powder C; and / or The concentration of the nitric acid aqueous solution is 8wt% to 15wt%, preferably 10wt% to 15wt%; the amount of the nitric acid aqueous solution is 0.8 to 1.1 times the weight of the powder C; and / or The calcination time is 3 to 6 hours.
6. The method for recycling a deactivated caprolactam hydrogenation catalyst according to claim 1, characterized in that: In step (5), the concentration of the phosphoric acid aqueous solution is 1 wt% to 3 wt%, preferably 1 wt% to 2 wt%; and the soaking time is 40 to 80 minutes.
7. The method for recycling a deactivated caprolactam hydrogenation catalyst according to claim 1, characterized in that: In step (6): the concentration of the nickel nitrate aqueous solution is expressed in grams of nickel nitrate per gram of water, and the specific calculation formula is: Wherein, a is the nickel content in the catalyst intermediate E (wt%); b is the water absorption rate of the catalyst intermediate E (wt%).
8. The method for recycling a deactivated caprolactam hydrogenation catalyst according to claim 1, characterized in that: In step (6): The catalyst intermediate E is immersed in the nickel nitrate aqueous solution for 40 to 80 minutes; and / or The calcination time is 3 to 6 hours.
9. The method for recycling a deactivated caprolactam hydrogenation catalyst according to claim 1, characterized in that: In step (7): The hydrogen reduction is carried out at 450-500°C.
10. The method for recycling a deactivated caprolactam hydrogenation catalyst according to claim 1, characterized in that: The drying steps are all carried out at 100-130°C.
Citation Information
Patent Citations
Method for regenerating catalyst in two-stage hydrogenation of cracked gasoline
CN104226378A
Activation and regeneration method of deactivated catalyst in process of synthesizing dimethyl oxalate by CO
CN106861775A
Regeneration method of deactivated hydrofining catalyst
CN112642443A
Preparation method of hydrotreating catalyst
CN114602485A
Recycling method of deactivated catalyst
CN116920878A