Method for separating and purifying desilicication product from red mud

Through multi-stage screening of red mud and dilute alkali removal treatment, high-purity desilicate products were successfully separated from red mud, solving the problem of difficult separation and resource utilization of desilicate products in red mud, and realizing red mud efficient decalcification and resource recycling.

CN118904529AActive Publication Date: 2024-11-08FUJIAN UNIV OF TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411127134.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-08
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

The prior art has failed to effectively separate and purify the desilicate product from red mud, resulting in the difficulty in analyzing and resource utilization of the complex mineral composition of red mud, and the desalination efficiency is low.

Method used

After drying the red mud, it is possible to perform coarse grinding and multi-stage reselection, and reselection of reselection concentrates with a density of less than 2.2 g/cm3, perform dilute alkali removal and solid-liquid separation, collect solid precipitates for rinsing and drying, and obtain The desilicate product purified product was used to shake the potassium hydroxide solution to remove impurities, and the original appearance and morphology of sodaite and calcium hyalite were retained.

Benefits of technology

High purity separation of desilicate products is achieved, the loss and operation costs are reduced, large-scale industrial applications are enabled, and raw materials are provided for scientific research and resource recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904529A_ABST
    Figure CN118904529A_ABST
Patent Text Reader

Abstract

The invention relates to a method for separating and purifying a desilicication product from red mud, which comprises the following steps: drying the red mud, coarsely grinding the red mud into a powdery material, sieving the powdery material through a 325-mesh vibrating screen, carrying out multi-stage reselection on the undersize product until reselected concentrate with the density of less than 2.2 g / cm < 3 > is selected, carrying out dilute alkali impurity removal on the obtained reselected concentrate, carrying out solid-liquid separation, and collecting a solid precipitate, thereby obtaining the desilicication product. And washing and drying the solid precipitate to obtain a purified desiliconized product. According to the method, the desilicication product is separated and purified from the red mud by adopting a simple method without adopting a high-temperature and high-pressure mode and the like, so that the original appearance forms and physicochemical properties of the desilicication products such as sodalite and cancrinite and the like are reserved to the greatest extent; the sample can be used as an original sample for scientific research to carry out mineralogical analysis, elemental composition analysis and micromorphology analysis on desiliconized products contained in the red mud. The separated and purified desiliconized product is high in purity, low in investment and operation cost and capable of being industrially applied on a large scale.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of harmless treatment and resource application of red mud, and specifically relates to a method for separating and purifying desiliconization products from red mud. Background Art

[0002] Red mud is a solid or semi-solid powdery mud waste discharged during the production of alumina. Due to its high salt and alkali content, strong corrosiveness, and certain radioactivity, its comprehensive utilization efficiency is low, and it is mainly stored in dams. The output of red mud varies depending on the ore grade, production process, and technical level. For every 1.0 ton of alumina produced, 0.8 to 2.0 tons of red mud will be discharged. When red mud is stored, it will cause serious ecological risks to the surrounding groundwater, surface water, soil, and atmospheric environment. Therefore, it is urgent to dispose of red mud harmlessly and as a resource.

[0003] When alumina is produced by the Bayer process, sintering process or combined process, silicon dioxide is easily supersaturated in the sodium aluminate solution and precipitates in the form of hydrated sodium aluminosilicate. The precipitate is called desiliconization product (DSPs). If DSPs precipitate during the dissolution process, they are present in the discharged red mud and cause Al2O3 and Na2O to be enriched in the red mud. The expression of DSPs in red mud is [Na2O·Al2O3·(1.68-1.85)SiO2]·nNa2X·qH2O, and the main mineral phase is sodalite 2NaX·[Na6Al6Si6O 24 ] and cancrystal 2CaCO3·[Na6Al6Si6O 24 If DSPs can be separated and purified from red mud, it will not only be beneficial to the qualitative and quantitative study of the mineral phases contained in the red mud, but also beneficial to the dealkalization of red mud and the resource utilization of red mud.

[0004] The mineral composition of red mud is extremely complex, including boehmite, gibbsite, quartz, calcite, goethite, hematite, rutile, anatase, DSPs and other minerals. When performing X-ray diffraction qualitative or quantitative analysis on the mineral phase of red mud, multiple peaks overlap and multiple similar diffraction peaks exist, making it difficult to analyze DSPs in red mud when multiple other minerals coexist. Therefore, it is necessary to separate and purify DSPs from the complex objects first, thereby reducing the complexity of energy spectrum analysis.

[0005] DSPs such as sodalite and cancrinite are also the main occurrence forms of solid alkaline minerals in red mud, and are the main source of chemically bound alkali in red mud, with extremely strong acid neutralization capacity (ANC). Compared with free alkalis such as sodium hydroxide and sodium carbonate that are easily soluble in the liquid phase in red mud, DSPs such as sodalite and cancrinite not only consume a large amount of acid or acid gas during the red mud dealkalization process, but also are easily left in the red mud due to incomplete dissolution and conversion, which ultimately affects the efficiency of red mud dealkalization.

[0006] DSPs such as sodalite and cancrystal can be separated and purified from red mud and can be used as resources. DSPs are not only rich in Al2O3 and Na2O, but can also be used as raw materials for recycling aluminum and sodium, and can also be made into products such as 4A zeolite, cryolite, and silica gel.

[0007] Currently, there is no efficient technology for extracting and purifying desiliconized products (DSPs) from red mud. Summary of the invention

[0008] In view of the above problems, the present invention provides a relatively simple method for separating and purifying desiliconization products from red mud, which does not require the use of high temperature and high pressure, and retains the original morphology and physical and chemical properties of desiliconization products such as sodalite and cancrystal to the greatest extent. The desiliconization products separated and purified by the present invention have high purity, low investment and operating costs, and can be applied on a large scale industrially.

[0009] The present invention is specifically implemented by the following technical scheme. According to the present invention, a method for separating and purifying desiliconization products from red mud comprises the following steps:

[0010] The red mud is dried and then coarsely ground into powdery material, which is then passed through a 325-mesh vibrating screen. The product under the screen is subjected to multi-stage gravity selection until the product with a density of less than 2.2 g / cm 3 The obtained gravity separation concentrate is subjected to dilute alkali impurity removal, and then solid-liquid separation is performed, the solid precipitate is collected, and the solid precipitate is rinsed and dried to obtain a desiliconized product purification product.

[0011] Furthermore, after passing through a 325-mesh vibrating screen, the particle size of the product on the screen is greater than 0.045 mm, mainly boehmite, gibbsite and quartz, and the particle size of the product under the screen is less than 0.045 mm, mainly desiliconization products (DSPs), calcite, goethite, hematite, rutile and anatase.

[0012] Furthermore, the main mineral components of the obtained gravity separation concentrate are desiliconization products (DSPs) and trace gibbsite, and the main mineral components of the gravity separation tailings are boehmite, hematite, goethite, rutile, anatase, quartz and calcite.

[0013] Furthermore, the specific method of removing impurities with dilute alkali on the obtained gravity separation concentrate includes: soaking the gravity separation concentrate in a potassium hydroxide solution with a concentration of not less than 1.2 mol / L, shaking or stirring to remove impurities, the impurity removal time is 80 to 120 minutes, and the liquid-solid ratio is 9:1 to 11:1. During the impurity removal process, the trace gibbsite in the gravity separation concentrate is dissolved in the dilute alkali solution, the gravity separation concentrate that has completed the impurity removal is separated into solid and liquid, and the concentrate is washed and dried to finally obtain a desiliconized product (DSPs) purified product.

[0014] Compared with the prior art, the present invention has obvious advantages and beneficial effects. By means of the above technical solution, the present invention can achieve considerable technical progress and practicality, and has a wide range of utilization value, and has at least the following advantages:

[0015] (1) The present invention uses a simple method to separate and purify the desiliconization products (DSPs) from red mud. The purified DSPs can be made into products such as 4A zeolite, cryolite, silica gel, etc., and aluminum and alkali can also be recovered therefrom. The separation and purification process of the present invention does not require the use of high temperature and high pressure, etc., and retains the original morphology and physical and chemical properties of the desiliconization products (DSPs) such as sodalite and cancryogenite to the greatest extent. It can be used as an original sample for scientific research to perform mineralogical analysis, elemental composition analysis, and microscopic morphology analysis on the DSPs contained in the red mud.

[0016] (2) The desiliconized products (DSPs) separated and purified by the method of the present invention are of high purity, with extremely low loss during the separation process, and no pressurization or calcination is used, so the investment and operation costs are low and can be applied on a large scale in industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is the SEM image of the DSPs purified product purified in Example 1.

[0018] Figure 2 This is the EDS spectrum of the DSPs purified product purified in Example 1. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] In the following examples, if no specific conditions are specified, all the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The raw materials and reagents used, if no manufacturer is specified, are all conventional products that can be purchased from the market.

[0021] Example 1

[0022] The red mud was dried in an oven at 60°C for 24 hours, and finely ground with a small ball mill to obtain a fine-grained powder material. The content of the material with a particle size of less than 0.150 mm in the powder material accounted for about 92% or more. The red mud powder material was passed through a 325-mesh vibrating screen. The product under the screen was passed through a primary spiral chute (the number of turns was 5, the outer radius was 150 mm, the inner radius was 35 mm, the pitch was 240 mm, the lateral inclination was 9°, and the inlet flow rate was set to 12.0 L / min) to obtain a primary gravity separation concentrate, and the primary gravity separation concentrate was passed through a secondary spiral chute (the number of turns was 5, the outer radius was 150 mm, the inner radius was 35 mm, the pitch was 240 mm, the lateral inclination was 9°, and the inlet flow rate was set to 5.0 L / min) to obtain a secondary gravity separation concentrate. The main mineral components of the secondary gravity separation concentrate were desiliconization products (DSPs) and trace gibbsite. 10 g of the secondary gravity concentrate was placed in a 100 mL potassium hydroxide solution with a concentration of 1.2 mol / L and stirred for 2 h. During the impurity removal process, the trace gibbsite in the secondary gravity concentrate was dissolved in the dilute alkali solution. The gravity concentrate that had completed the impurity removal was subjected to solid-liquid separation. The impurity-removed concentrate was collected and rinsed with deionized water, and dried in an oven to obtain a DSPs purified product.

[0023] Figure 1 and Figure 2 They are the SEM microscopic morphology and EDS energy spectrum of the purified DSPs product. From the mineral element composition and occurrence state, it can be seen that the purified product is mainly desiliconization products cancrinite and sodalite.

[0024] Example 2

[0025] The red mud was dried in an oven at 80°C for 20 hours, and finely ground with a small ball mill to obtain a fine-grained powder material. The content of the material with a particle size of less than 0.150 mm in the powder material accounted for about 90% or more. The red mud powder material was passed through a 325-mesh vibrating screen. The product under the screen passed through a primary spiral chute (the number of turns was 5, the outer radius was 150 mm, the inner radius was 35 mm, the pitch was 240 mm, the lateral inclination was 9°, and the inlet flow rate was set to 12.0 L / min) to obtain a primary gravity separation concentrate, and the primary gravity separation concentrate was passed through a secondary spiral chute (the number of turns was 5, the outer radius was 150 mm, the inner radius was 35 mm, the pitch was 240 mm, the lateral inclination was 9°, and the inlet flow rate was set to 5.0 L / min) to obtain a secondary gravity separation concentrate. The main mineral components of the secondary gravity separation concentrate were desiliconization products (DSPs) and trace gibbsite. 10g of secondary gravity concentrate was placed in a 110mL potassium hydroxide solution with a concentration of 1.5mol / L and stirred for 2h. During the impurity removal process, the trace gibbsite in the secondary gravity concentrate was dissolved in the dilute alkali solution. The gravity concentrate that had completed the impurity removal was subjected to solid-liquid separation. The concentrate after impurity removal was collected and rinsed with deionized water, and dried in an oven to obtain DSPs purified product.

[0026] Example 3

[0027] The red mud was dried in an oven at 70°C for 24 hours, and finely ground with a small ball mill to obtain a fine-grained powder material. The content of the material with a particle size of less than 0.150 mm in the powder material accounted for about 93% or more. The red mud powder material was passed through a 325-mesh vibrating screen. The product under the screen passed through a primary spiral chute (the number of turns was 5, the outer radius was 150 mm, the inner radius was 35 mm, the pitch was 240 mm, the lateral inclination was 9°, and the inlet flow rate was set to 12.0 L / min) to obtain a primary gravity separation concentrate, and the primary gravity separation concentrate was passed through a secondary spiral chute (the number of turns was 5, the outer radius was 150 mm, the inner radius was 35 mm, the pitch was 240 mm, the lateral inclination was 9°, and the inlet flow rate was set to 5.0 L / min) to obtain a secondary gravity separation concentrate. The main mineral components of the secondary gravity separation concentrate are desiliconization products (DSPs) and trace gibbsite. 10g of secondary gravity concentrate was placed in a 90mL potassium hydroxide solution with a concentration of 1.3mol / L and stirred for 2h. During the impurity removal process, the trace gibbsite in the secondary gravity concentrate was dissolved in the dilute alkali solution. The gravity concentrate that had completed the impurity removal was subjected to solid-liquid separation. The concentrate after impurity removal was collected and rinsed with deionized water, and dried in an oven to obtain the DSPs purified product.

[0028] The above is only an embodiment of the present invention, and does not limit the present invention in any form. The present invention can also have other forms of embodiments according to the above structures and functions, which are not listed one by one. Therefore, any simple modification, equivalent change and modification made by any technician familiar with the profession to the above embodiment according to the technical essence of the present invention without departing from the scope of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A method for separating and purifying desiliconization products from red mud, It is characterized in that The following steps are involved: The red mud is dried and then coarsely ground into powdery material, which is then passed through a 325-mesh vibrating screen. The product under the screen is subjected to multi-stage gravity selection until the product with a density of less than 2.2 g / cm 3 The obtained gravity separation concentrate is subjected to dilute alkali impurity removal, and then solid-liquid separation is performed, the solid precipitate is collected, and the solid precipitate is rinsed and dried to obtain a desiliconized product purification product.

2. The method for separating and purifying desiliconized products from red mud according to claim 1, It is characterized in that After passing through a 325-mesh vibrating screen, the particle size of the product on the screen is greater than 0.045 mm, mainly boehmite, gibbsite and quartz, and the particle size of the product under the screen is less than 0.045 mm, mainly desiliconization products, calcite, goethite, hematite, rutile and anatase.

3. The method for separating and purifying desiliconized products from red mud according to claim 1, It is characterized in that The main mineral components of the obtained gravity separation concentrate are desiliconization products and trace amounts of gibbsite.

4. The method for separating and purifying desiliconized products from red mud according to claim 1 or 3, It is characterized in that The specific method of removing impurities with dilute alkali on the obtained gravity separation concentrate includes: soaking the gravity separation concentrate in a potassium hydroxide solution with a concentration of not less than 1.2 mol / L for shaking or stirring for 80 to 120 minutes, and the liquid-to-solid ratio is 9:1 to 11:1.

Citation Information

Patent Citations

  • Processing method of separating fine red mud

    CN105478218A

  • Separation method for extracting iron and removing sodium from red mud

    CN108686828A

  • Method for reducing alkalinity of red mud by utilizing industrial wastes

    CN109530392A

  • Comprehensive utilization method and device for red mud

    CN112547753A

  • Comprehensive utilization method for high-iron low-silicon red mud

    CN112808755A