Surface cleaning method for corrosion-resistant delayed-fracture-resistant high-strength nut

Through multi-step treatment such as pretreatment, rust removal, ultrasonic cleaning and vibration cleaning, combined with composite cleaning agent, the strength and corrosion resistance of the nut are significantly improved, and the performance of nuts in the existing technology under high stress and corrosive environments is solved. Improvement issues are suitable for large-scale production and are economically beneficial.

CN118904810AInactive Publication Date: 2024-11-08HAIYAN FUHONG FASTENING CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411015351.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art still has room for improvement in improving the overall strength, resistance to delay fracture and corrosion resistance of nuts, especially in nuts working under high stress and corrosive environments, where effective surface treatment methods are lacking.

Method used

Heat and quickly cool the nuts by pretreatment steps, combining mechanical or chemical rust removal, ultrasonic cleaning, vibration cleaning and composite cleaning agent treatment, including pretreatment, rust removal, initial drying, ultrasonic cleaning, re-drying, vibration cleaning and final Dry and finally carry out quality testing.

Benefits of technology

It significantly improves the strength and resistance to delay fracture, improves corrosion resistance, simplifies the cleaning process, is suitable for large-scale production and has good economic and social benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904810A_ABST
    Figure CN118904810A_ABST
Patent Text Reader

Abstract

The invention discloses a corrosion-resistant delayed-fracture-resistant high-strength nut surface cleaning method which comprises the following steps: a pretreatment step: placing a to-be-treated nut in heating equipment, heating to a preset temperature, and preserving heat, so that microstructure change occurs in a nut material, and the mechanical property of the nut material is enhanced; then the heated nut is rapidly cooled to the room temperature, the strength and delayed fracture resistance of the nut are further improved, and the pretreated nut is obtained; rust removal treatment is conducted, specifically, the pretreated nut is placed in rust removal equipment, and a rust layer and impurities on the surface are preliminarily removed through a mechanical or chemical method; the method has the beneficial effects that through the unique pretreatment step, the strength and delayed fracture resistance of the nut are remarkably enhanced; a multi-step cleaning and drying process is combined with the use of a composite cleaning agent, so that the corrosion resistance of the nut is effectively improved; ultrasonic cleaning and vibration cleaning are combined, so that the cleaning speed is greatly increased, the decontamination effect is greatly improved, and the follow-up treatment difficulty is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nut surface cleaning, and in particular relates to a method for cleaning the surface of a corrosion-resistant, delayed-fracture-resistant, high-strength nut. Background Art

[0002] The primary purpose of cleaning nuts is to remove dirt on their surface, such as dust, grease, paint, coatings, and residual cooling oil, coolant, rust-proof liquid and other attachments from the previous process; these dirt not only affect the appearance of the nuts, but may also affect their performance; through cleaning, the smoothness of the nut surface is improved, which is conducive to subsequent assembly and use; the surface of the nut after cleaning is cleaner, which is conducive to achieving a better friction coefficient during installation, improving the tightness and stability of the connection; cleaning can remove impurities on the nut surface, reduce the jamming and wear caused by the threaded connection, and thus extend the service life of the nut.

[0003] A cleaning method for slotted thin plate nuts with publication number CN109396096A discloses placing the slotted thin plate nuts at the beginning of the conveyor belt; the slotted thin plate nuts are preliminarily cleaned with cleaning liquid in the cleaning liquid spraying section to obtain pre-cleaned parts; the pre-cleaned parts are deeply cleaned with cleaning liquid in the ultrasonic cleaning section to obtain deeply cleaned parts; the first anti-rust liquid spraying section is preliminarily sprayed with anti-rust liquid with anti-rust liquid to obtain primary anti-rust parts; the primary anti-rust parts are primarily dried in the first high-temperature drying section to obtain primary dried parts; the primary dried parts are secondarily sprayed with anti-rust liquid with anti-rust liquid in the second anti-rust liquid spraying section; the secondary anti-rust parts are secondarily dried in the second high-temperature drying section to obtain secondary dried parts; the secondary dried parts are sprayed with anti-rust oil in the anti-rust spraying section to obtain rust-proof finished parts; the rust-proof finished parts are blow-dried in the blowing section to obtain final parts;

[0004] In the prior art, although the surface cleaning and rust prevention of nuts are achieved through multi-step treatments such as cleaning, rust prevention, and drying, there is still room for improvement in improving the overall strength of the nuts, resistance to delayed fracture, and further enhancing corrosion resistance. In particular, nuts working in high stress and corrosive environments are in urgent need of a more effective surface treatment method. Summary of the invention

[0005] The purpose of the present invention is to provide a method for cleaning the surface of a corrosion-resistant and delayed-fracture-resistant high-strength nut, which can significantly improve the strength and corrosion resistance of the nut and enhance its delayed-fracture resistance.

[0006] To achieve the above object, the present invention provides the following technical solution: a method for cleaning the surface of a corrosion-resistant, delayed-fracture-resistant, high-strength nut, comprising:

[0007] Pretreatment step: placing the nut to be treated in a heating device, heating it to a predetermined temperature, and keeping it warm, so that the microstructure inside the nut material changes and its mechanical properties are enhanced; then the heated nut is quickly cooled to room temperature to further improve the strength and delayed fracture resistance of the nut, thereby obtaining a pretreated nut;

[0008] Rust removal: Place the pretreated nuts in the rust removal equipment and use mechanical or chemical methods to preliminarily remove the surface rust layer and impurities. During the rust removal process, add rust remover to improve the rust removal effect and ensure that the nut surface is clean and rust-free.

[0009] Initial drying: The rust-removed nuts are initially dried to remove surface moisture;

[0010] Ultrasonic cleaning: Place the nuts after initial drying in an ultrasonic cleaning machine and add a cleaning solution containing a metal cleaning agent for deep cleaning;

[0011] Re-drying: Re-dry the nuts after ultrasonic cleaning to ensure that the surface is completely dry;

[0012] Vibration cleaning and compound cleaning agent treatment: Place the re-dried nuts in the cleaning basket or cleaning rack of the vibration cleaning machine and immerse them in the cleaning solution containing the compound cleaning agent;

[0013] Final drying and testing: The nuts after vibration cleaning are finally dried to ensure that the surface is completely dry; the quality of the processed nuts is tested to ensure that they meet the design requirements.

[0014] As a preferred technical solution of the present invention, the quality inspection includes a corrosion resistance test and a delayed fracture resistance test.

[0015] As a preferred technical solution of the present invention, the predetermined temperature is 200-300° C. and the temperature is kept for 10-20 minutes.

[0016] As a preferred technical solution of the present invention, the rust remover is one of phosphoric acid and hydrochloric acid.

[0017] As a preferred technical solution of the present invention, the metal cleaning agent is prepared from the following raw materials: 30-40% sodium silicate, 40-50% sodium tripolyphosphate, and the balance is fatty alcohol polyoxyethylene ether.

[0018] As a preferred technical solution of the present invention, the composite cleaning agent is prepared from a surfactant, a high-efficiency builder and a corrosion inhibitor.

[0019] As a preferred technical solution of the present invention, the high-efficiency builder is one of phosphate, silicate and carbonate.

[0020] As a preferred technical solution of the present invention, the corrosion inhibitor is zinc naphthenate.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] Through a unique pre-treatment step, the strength and delayed fracture resistance of the nut are significantly enhanced;

[0023] The multi-step cleaning and drying process, combined with the use of composite cleaning agents, effectively improves the corrosion resistance of the nuts;

[0024] The combination of ultrasonic cleaning and vibration cleaning greatly improves the cleaning speed and decontamination effect, and reduces the difficulty of subsequent processing;

[0025] The operation is simple, suitable for large-scale production, and has good economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a flow chart of the cleaning method of the present invention. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] Example 1

[0029] See also Figure 1 , which is the first embodiment of the present invention, provides a method for cleaning the surface of a corrosion-resistant, delayed-fracture-resistant, high-strength nut, comprising:

[0030] Pretreatment step: placing the nut to be treated in a heating device, heating it to a predetermined temperature of 200°C, and keeping it warm for 10 minutes, so that the microstructure inside the nut material changes and its mechanical properties are enhanced; then the heated nut is quickly cooled to room temperature, and the strength and delayed fracture resistance of the nut are further improved through the rapid hot and cold treatment (quenching) effect, so as to obtain a pretreated nut;

[0031] Rust removal: The pretreated nuts are placed in the rust removal equipment, and the surface rust layer and impurities are initially removed by mechanical methods. During the rust removal process, rust remover is added to improve the rust removal effect and ensure that the nut surface is clean and rust-free; the rust remover is phosphoric acid;

[0032] Initial drying: The rust-removed nuts are initially dried to remove surface moisture;

[0033] Ultrasonic cleaning: Place the nuts after initial drying in an ultrasonic cleaning machine and add a cleaning solution containing a metal cleaning agent for deep cleaning; the cavitation effect of ultrasound can effectively remove tiny particles and residues;

[0034] Re-drying: Re-dry the nuts after ultrasonic cleaning to ensure that the surface is completely dry;

[0035] Vibration cleaning and composite cleaning agent treatment: put the nuts that have been dried again on the cleaning rack of the vibration cleaning machine and immerse them in the cleaning liquid containing the composite cleaning agent; the vibration of the vibration cleaning machine further enhances the cleaning effect to ensure that the surface of the nuts is thoroughly cleaned; the composite cleaning agent is formulated with Tomamine AO-455 surfactant, high-efficiency builder and corrosion inhibitor; this cleaning agent can not only significantly improve the cleaning speed and decontamination effect, but also effectively protect the surface of the nuts from corrosion; Tomamine AO-455 is a multifunctional surfactant of the ultra-low-foaming amine oxide type with excellent detergency; it is suitable for alkaline or acidic hard surface cleaning formulas, especially for conditions that require low or no foam; Tomamine AO-455 has excellent performance in cleaning speed, environmental protection and safety, and is compatible with anionic, nonionic and cationic surfactants; the high-efficiency builder is phosphate; the corrosion inhibitor is zinc cyclohexaneate;

[0036] Final drying and testing: The nuts after vibration cleaning are finally dried to ensure that the surface is completely dry; the treated nuts are quality tested, including corrosion resistance test and delayed fracture resistance test, to ensure that they meet the design requirements.

[0037] In this embodiment, preferably, the metal cleaning agent is prepared from the following raw materials: 30% sodium silicate, 40% sodium tripolyphosphate, and the balance is fatty alcohol polyoxyethylene ether; the preparation method is to put the above components into a stirrer in proportion and stir and mix them, and after stirring and mixing evenly, package them to obtain the obtained product; when using, take this product and water in a ratio of 1:10, dissolve them and it can be used to clean metal.

[0038] Example 2

[0039] See also Figure 1 , which is the second embodiment of the present invention, provides a method for cleaning the surface of a corrosion-resistant, delayed-fracture-resistant, high-strength nut, comprising:

[0040] Pretreatment step: placing the nut to be treated in a heating device, heating it to a predetermined temperature of 250°C, and keeping it warm for 15 minutes, so that the microstructure inside the nut material changes and its mechanical properties are enhanced; then the heated nut is quickly cooled to room temperature, and the strength and delayed fracture resistance of the nut are further improved through the rapid hot and cold treatment (quenching) effect, so as to obtain a pretreated nut;

[0041] Rust removal: Place the pretreated nuts in the rust removal equipment and use chemical methods to preliminarily remove the surface rust layer and impurities. During the rust removal process, add rust remover to improve the rust removal effect and ensure that the nut surface is clean and rust-free; the rust remover is hydrochloric acid;

[0042] Initial drying: The rust-removed nuts are initially dried to remove surface moisture;

[0043] Ultrasonic cleaning: Place the nuts after initial drying in an ultrasonic cleaning machine and add a cleaning solution containing a metal cleaning agent for deep cleaning; the cavitation effect of ultrasound can effectively remove tiny particles and residues;

[0044] Re-drying: Re-dry the nuts after ultrasonic cleaning to ensure that the surface is completely dry;

[0045] Vibration cleaning and compound cleaning agent treatment: put the nuts that have been dried again into the cleaning basket of the vibration cleaning machine and immerse them in the cleaning liquid containing the compound cleaning agent; the vibration of the vibration cleaning machine further enhances the cleaning effect to ensure that the surface of the nuts is thoroughly cleaned; the compound cleaning agent is formulated with Tomamine AO-455 surfactant, high-efficiency builder and corrosion inhibitor; this cleaning agent can not only significantly improve the cleaning speed and decontamination effect, but also effectively protect the surface of the nuts from corrosion; Tomamine AO-455 is a multifunctional surfactant of the ultra-low-foaming amine oxide type with excellent detergency; it is suitable for alkaline or acidic hard surface cleaning formulas, especially for conditions that require low or no foam; Tomamine AO-455 has excellent performance in cleaning speed, environmental protection and safety, and is compatible with anionic, nonionic and cationic surfactants; the high-efficiency builder is silicate; the corrosion inhibitor is zinc cyclohexaneate;

[0046] Final drying and testing: The nuts after vibration cleaning are finally dried to ensure that the surface is completely dry; the treated nuts are quality tested, including corrosion resistance test and delayed fracture resistance test, to ensure that they meet the design requirements.

[0047] In this embodiment, preferably, the metal cleaning agent is prepared from the following raw materials: 35% sodium silicate, 45% sodium tripolyphosphate, and the balance is fatty alcohol polyoxyethylene ether; the preparation method is to put the above components into a stirrer in proportion and stir and mix them, and after stirring and mixing evenly, package them to obtain the obtained product; when using, take this product and water in a ratio of 1:10, dissolve them and it can be used to clean metal.

[0048] Example 3

[0049] See also Figure 1 , which is the third embodiment of the present invention, provides a method for cleaning the surface of a corrosion-resistant, delayed-fracture-resistant, high-strength nut, comprising:

[0050] Pretreatment step: placing the nut to be treated in a heating device, heating it to a predetermined temperature of 300°C, and keeping it warm for 20 minutes, so that the microstructure inside the nut material changes and its mechanical properties are enhanced; then the heated nut is quickly cooled to room temperature, and the strength and delayed fracture resistance of the nut are further improved through the rapid hot and cold treatment (quenching) effect, so as to obtain a pretreated nut;

[0051] Rust removal: The pretreated nuts are placed in the rust removal equipment, and the surface rust layer and impurities are initially removed by mechanical methods. During the rust removal process, rust remover is added to improve the rust removal effect and ensure that the nut surface is clean and rust-free; the rust remover is phosphoric acid;

[0052] Initial drying: The rust-removed nuts are initially dried to remove surface moisture;

[0053] Ultrasonic cleaning: Place the nuts after initial drying in an ultrasonic cleaning machine and add a cleaning solution containing a metal cleaning agent for deep cleaning; the cavitation effect of ultrasound can effectively remove tiny particles and residues;

[0054] Re-drying: Re-dry the nuts after ultrasonic cleaning to ensure that the surface is completely dry;

[0055] Vibration cleaning and compound cleaning agent treatment: put the nuts that have been dried again into the cleaning basket of the vibration cleaning machine and immerse them in the cleaning liquid containing the compound cleaning agent; the vibration of the vibration cleaning machine further enhances the cleaning effect to ensure that the surface of the nuts is thoroughly cleaned; the compound cleaning agent is formulated with Tomamine AO-455 surfactant, high-efficiency builder and corrosion inhibitor; this cleaning agent can not only significantly improve the cleaning speed and decontamination effect, but also effectively protect the surface of the nuts from corrosion; Tomamine AO-455 is a multifunctional surfactant of the ultra-low-foaming amine oxide type with excellent detergency; it is suitable for alkaline or acidic hard surface cleaning formulas, especially for conditions that require low or no foam; Tomamine AO-455 has excellent performance in cleaning speed, environmental protection and safety, and is compatible with anionic, nonionic and cationic surfactants; the high-efficiency builder is carbonate; the corrosion inhibitor is zinc cyclohexaneate;

[0056] Final drying and testing: The nuts after vibration cleaning are finally dried to ensure that the surface is completely dry; the treated nuts are quality tested, including corrosion resistance test and delayed fracture resistance test, to ensure that they meet the design requirements.

[0057] In this embodiment, preferably, the metal cleaning agent is prepared from the following raw materials: 40% sodium silicate, 50% sodium tripolyphosphate, and the balance is fatty alcohol polyoxyethylene ether; the preparation method is to put the above components into a stirrer in proportion and stir and mix them, and after stirring and mixing evenly, package them to obtain the obtained product; when using, take this product and water in a ratio of 1:10, dissolve them and it can be used to clean metal.

[0058] Although the embodiments of the present invention have been shown and described, as detailed above, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for cleaning the surface of a corrosion-resistant, delayed-fracture-resistant, high-strength nut, characterized in that: The method comprises the following steps: placing the nut to be treated in a heating device, heating it to a predetermined temperature, and keeping the temperature, so that the microstructure inside the nut material changes and its mechanical properties are enhanced; then rapidly cooling the heated nut to room temperature, further improving the strength and delayed fracture resistance of the nut, and obtaining a pretreated nut; Rust removal: Place the pretreated nuts in the rust removal equipment and use mechanical or chemical methods to preliminarily remove the surface rust layer and impurities. During the rust removal process, add rust remover to improve the rust removal effect and ensure that the nut surface is clean and rust-free. Initial drying: The rust-removed nuts are initially dried to remove surface moisture; Ultrasonic cleaning: Place the nuts after initial drying in an ultrasonic cleaning machine and add a cleaning solution containing a metal cleaning agent for deep cleaning; Re-drying: Re-dry the nuts after ultrasonic cleaning to ensure that the surface is completely dry; Vibration cleaning and compound cleaning agent treatment: Place the re-dried nuts in the cleaning basket or cleaning rack of the vibration cleaning machine and immerse them in the cleaning solution containing the compound cleaning agent; Final drying and testing: The nuts after vibration cleaning are finally dried to ensure that the surface is completely dry; the quality of the processed nuts is tested to ensure that they meet the design requirements.

2. A method for cleaning the surface of a corrosion-resistant, delayed-fracture-resistant, high-strength nut according to claim 1, characterized in that: The quality inspection includes a corrosion resistance test and a delayed fracture resistance test.

3. The method for cleaning the surface of a corrosion-resistant, delayed-fracture-resistant, high-strength nut according to claim 1, characterized in that: The predetermined temperature is 200-300° C. and the temperature is kept for 10-20 minutes.

4. The method for cleaning the surface of a corrosion-resistant, delayed-fracture-resistant, high-strength nut according to claim 1, characterized in that: The rust remover is one of phosphoric acid and hydrochloric acid.

5. The method for cleaning the surface of a corrosion-resistant, delayed-fracture-resistant, high-strength nut according to claim 1, characterized in that: The metal cleaning agent is prepared from the following raw materials: 30-40% of sodium silicate, 40-50% of sodium tripolyphosphate, and the balance of fatty alcohol polyoxyethylene ether.

6. The method for cleaning the surface of a corrosion-resistant, delayed-fracture-resistant, high-strength nut according to claim 1, characterized in that: The composite cleaning agent is prepared from a surfactant, a high-efficiency builder and a corrosion inhibitor.

7. A method for cleaning the surface of a corrosion-resistant, delayed-fracture-resistant, high-strength nut according to claim 6, characterized in that: The high-efficiency builder is one of phosphate, silicate and carbonate.

8. The method for cleaning the surface of a corrosion-resistant, delayed-fracture-resistant, high-strength nut according to claim 6, characterized in that: The corrosion inhibitor is zinc naphthenate.

Citation Information

Patent Citations

  • Cleaning method for slotted type sheet nut

    CN109396096A