Forging method for continuous die forging of boss forge piece

By designing the mold and forging process, the problems of energy waste and extended production cycle caused by burrs on forgings were solved, realizing continuous die forging production of boss forgings, improving production efficiency and saving energy.

CN118905129AActive Publication Date: 2024-11-08CHINA NAT ERZHONG GRP DEYANG WANHANG DIE FORGING CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411219369.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-08
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

When forging high-strength steel forgings, the presence of burrs during the die forging process leads to energy waste and extended production cycles. This is especially true in the continuous die forging of boss forgings, where the presence of burrs hinders metal flow, resulting in incomplete filling of the cavity and requiring additional cooling and cutting to remove the burrs.

Method used

By designing the mold and forging process, the edge trimming mold design of die forging 1 fire and die forging 2 fire is adopted. First, the burrs in the easy-to-fill areas are removed under hot conditions, while the burrs in the difficult-to-fill areas are retained. Forging is carried out using a mold made of 5CrMnMo material and a 10-ton die forging hammer. Combined with alloy steel glass protective lubricant and numerical simulation, continuous production of forgings is realized.

Benefits of technology

It enables continuous production of forgings, saves energy and production cycle, improves production efficiency, reduces forming tonnage requirements, and avoids the energy waste of traditional cutting and deburring.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905129A_ABST
    Figure CN118905129A_ABST
Patent Text Reader

Abstract

The invention provides a forging method for continuous die forging of a boss forge piece. The forging method comprises the following steps: 1, designing; the method comprises the following steps: S1, finding out an unfilled place of a forge piece in a forming process through rough blank design, mold design and numerical simulation; s2, matching design of a die forging first flame trimming die is carried out; s3, the forge piece is directly returned to the furnace after the first die forging fire; 2, forging; k1, uniformly spraying an alloy steel glass protective lubricant on the manufactured blank, and then heating in a natural gas furnace; k2, die forging first fire, wherein the preheating temperature of the die is 350 DEG C, and the preheating time is longer than or equal to 12 hours; k3, the forge piece is transferred to a die forging first flame trimming die to be trimmed; k4, the hot forged piece obtained after edge cutting is returned to the furnace to be heated; k5, die forging fire 2, wherein a die for die forging fire 1 is adopted; and K6, the forge piece is transferred to a second die forging flame trimming die to be trimmed. The problem that the forge piece must be cooled to remove redundant burrs after first hot die forging is solved, and the purposes of continuous production and efficiency improvement are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of forging high-strength steel forgings for aircraft, in particular to a forging method for continuous die forging of boss forgings. Background Art

[0002] High-strength steel is widely used in the automotive industry, machinery manufacturing, aerospace and other fields, and is usually used to manufacture key structural components with high strength and high toughness. High-strength steel has high hardenability and good toughness and plasticity. In industrial production, it is often used to produce some parts that require both strength and the ability to withstand impact and alternating loads. However, it has the characteristics of high deformation resistance and difficult metal flow during forging production.

[0003] Taking the second generation high strength steel 30CrNi4MoA forgings for aircraft as an example, the initial forging temperature of the forging is generally controlled at 1150-1200℃ to ensure that the material has good plasticity; the final forging temperature is controlled at 850-900℃ to avoid forging cracks caused by too low temperature; and the deformation of each forging needs to be reasonably controlled to avoid excessive deformation causing internal defects in the material. During the die forging process, due to the large cross-sectional changes, when the high package position is not full, wider burrs have appeared in other places, resulting in excessive deformation resistance. At this time, the burrs need to be removed before the second die forging; the forging needs to be cooled down during production. Figure 1 The cutting line uses flame cutting to remove burrs, and then the forgings are heated and forged, which results in energy waste and longer production cycles.

[0004] If the trimming die is used to completely remove the burrs of the forging, such as Figure 2 According to the numerical simulation shown in the figure, the upper die and the lower die are closed during the second die forging (i.e., the underpressure is 0 mm), and the high part of the forging is not fully filled. Figure 3 As shown in the figure; because the existence of burrs can hinder the outward flow of metal, more metal is used to fill the cavity; after removing the burrs, part of the metal flows outward due to the minimum resistance, thus flowing outward to form burrs, resulting in less metal in the cavity and making the forging incompletely filled. Summary of the invention

[0005] The technical problem solved by the present invention is to provide a forging method for continuous die forging of boss forgings, which solves the problem that the forgings must be cooled to remove excess burrs after the first die forging, thereby achieving the purpose of continuous production and improving efficiency.

[0006] The technical solution adopted by the present invention to solve its technical problem is:

[0007] A forging method for continuous die forging of a boss forging comprises the following steps:

[0008] 1. Design

[0009] S1. Through blank design, die design and numerical simulation, find out the places where the forging is not filled during the forming process;

[0010] S2, performing matching design of die forging 1 fire trimming die, in which the female die of die forging 1 fire trimming die is designed, the forging is positioned in the female die through the positioning position to perform positioning trimming, and the burrs are cut off;

[0011] S3, after die forging 1 fire, the forgings are directly returned to the furnace;

[0012] 2. Forging

[0013] K1. Spray the manufactured blank evenly with alloy steel glass protective lubricant, and then heat it in a natural gas furnace at a heating temperature of 1150-1180°C and a heating coefficient of 0.3-0.6;

[0014] K2, die forging 1 fire: die preheating temperature 350 ℃, preheating time ≥ 12 hours, put the heated blank into the cavity, straighten and level it, hit it lightly 1-2 times, lift the forging to blow off the oxide scale and then hit it hard to form, control the underpressure 10-20mm, and control the final forging temperature ≥ 850 ℃;

[0015] K3. Transfer the forging to the die forging 1 fire trimming die for trimming, and the trimming temperature is ≥800℃;

[0016] K4. Return the hot forgings after trimming to the furnace for heating at a temperature of 1150-1180°C and a heating coefficient of 0.15-0.4;

[0017] K5, Die forging 2 fires: Still use the die forging 1 fire, the cavity temperature ≥ 200℃. Put the heated billet into the cavity, straighten and level it, hit it lightly 1-2 times, lift the forging to blow off the oxide scale and then hit it hard to form, control the underpressure to meet the requirements of the drawing, and control the final forging temperature ≥ 850℃;

[0018] K6. Transfer the forging to the die forging 2-fire trimming die for trimming. The trimming temperature is ≥800℃. After trimming, the forging is corrected.

[0019] In step S1, the mold design includes a side bridge portion having a thickness of 4 to 8 mm and a width of 12 to 20 mm, and a rough edge bin portion having a thickness of 15 to 30 mm and a width of 50 to 80 mm.

[0020] The die is made of 5CrMnMo material. The die is used to forge the forgings by a 10-ton die forging hammer. The heating temperature of the forging blank is 1150-1180° C. The hot forging digital die is designed and manufactured according to the forging shrinkage rate of 1.5%.

[0021] In step S1, the blank is designed according to the forging shape, and the burr weight and fire consumption are added by calculating the weight.

[0022] In step S2, a width of 5 to 15 mm is reserved in the design of the female die of the die forging 1 fire trimming die.

[0023] In step K3, the trimming is performed by a punch, and the punch includes a cylindrical end head with a half-wrapped structure.

[0024] The beneficial effects of the present invention are:

[0025] 1. By completely removing the burrs in the places where the cavity is easy to fill, the tonnage required for forming is reduced; the burrs in the places where the cavity is difficult to fill are retained to hinder the outward flow of metal, which is conducive to filling the cavity with blanks; by completing the partitioning and storage of the above burrs in the hot state of the forging, continuous production of forgings can be achieved, saving energy and cycle. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The cutting line diagram of the forging to be deburred;

[0027] Figure 2 This is the forging picture after being completely trimmed;

[0028] Figure 3 This is the forging picture after the second die forging;

[0029] Figure 4 This is a simulation diagram of the unfilled position during the forging process;

[0030] Figure 5 This is the design drawing of the female die of the die forging 1 fire trimming die;

[0031] Figure 6 This is a physical picture of the forging after trimming on the die forging 1 fire trimming die;

[0032] Figure 7 This is a physical picture of the burrs after trimming on the die forging 1 fire trimming die;

[0033] Figure 8 It is a schematic diagram of the appearance structure of the forging;

[0034] Fig. 9 This is a schematic diagram of the rough structure. DETAILED DESCRIPTION

[0035] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0036] Example 1

[0037] A forging method for continuous die forging of a boss forging comprises the following steps:

[0038] 1. Design

[0039] S1. Through blank design, die design and numerical simulation, find out the places where the forging is not filled during the forming process, such as Figure 4 As shown, it can be seen that the difficult-to-fill area is the high package, where there are fewer burrs;

[0040] S2, such as Figure 5 As shown, the matching design of die forging 1 fire trimming die is carried out. In the design of the female die of die forging 1 fire trimming die, the forging is positioned and trimmed in the female die through the positioning position. The cutting edge of the boss position (the cutting edge of the female die of die forging 1 fire trimming die and the convex part of the cutting edge of the female die of die forging 2 fire trimming die) needs to be 1 to 2 times the width of the burr groove bridge part, designed into a triangle with a smooth transition, and the burrs are cut off to prevent the occurrence of burr stacking and spring damage in the design of traditional trimming dies.

[0041] S3, such as Figure 6 As shown in the figure, after die forging 1, the forgings are directly returned to the furnace, which saves energy costs, eliminates the intermediate process of flame cutting, and improves production efficiency;

[0042] 2. Forging

[0043] K1. Spray the manufactured blank evenly with alloy steel glass protective lubricant, and then heat it in a natural gas furnace at a heating temperature of 1150-1180°C and a heating coefficient of 0.3-0.6;

[0044] K2, Die forging 1 fire: Die preheating temperature 350℃, preheating time ≥12 hours, put the heated billet into the cavity, straighten and level it, first lightly strike (forgings are produced with a 10-ton die forging hammer, the light strike pressure range is 2-5 tons) 1-2 hammers, lift the forging to blow off the oxide scale and then hit it hard (the heavy strike pressure range is 7-10 tons) to form, control the underpressure to 10-20mm, and control the final forging temperature ≥850℃;

[0045] Light tapping can position the blank, prevent it from flying off, and break off the oxide scale. After the oxide scale is blown away, heavy tapping can make the blank quickly form within the deformation temperature of the material, which is conducive to filling.

[0046] K3, such as Figure 6 As shown, the forging is transferred to the die forging 1 fire trimming die for trimming, and the trimming temperature is ≥800℃. Figure 7 As shown, it can be seen that the burrs are trimmed in the middle, eliminating the possibility of sticking to the punch, and the burrs at the high burrs are retained, which is conducive to the forming and filling of the forgings;

[0047] K4. Return the hot forgings after trimming to the furnace for heating at a temperature of 1150-1180°C and a heating coefficient of 0.15-0.4;

[0048] K5, Die forging 2 fires: still use the die forging 1 fire, the cavity temperature ≥ 200℃; put the heated billet into the cavity, straighten and level it, first lightly hit (the pressure range of light hitting is 2-5 tons) 1-2 hammers, lift the forging to blow off the oxide scale and then hit it hard (the pressure range of heavy hitting is 7-10 tons) to form, control the underpressure to meet the requirements of the drawing, and control the final forging temperature ≥ 850℃;

[0049] K6. Transfer the forging to the die forging 2-fire trimming die for trimming. The trimming temperature is ≥800℃. After trimming, the forging is corrected.

[0050] In step S1, the mold design includes a side bridge portion having a thickness of 4 to 8 mm and a width of 12 to 20 mm, and a rough edge bin portion having a thickness of 15 to 30 mm and a width of 50 to 80 mm.

[0051] The die is made of 5CrMnMo material. The die is used to forge the forgings by a 10-ton die forging hammer. The heating temperature of the forging blank is 1150-1180° C. The hot forging digital die is designed and manufactured according to the forging shrinkage rate of 1.5%.

[0052] In step S1, Figures 8 to 9 As shown, the blank is designed according to the forging shape, and the blank is designed to be as simple and easy to operate as possible. The weight is calculated by adding the burr weight and the fire consumption, and simulation software can be used to assist the design.

[0053] The weight calculation formula is: blanking weight = forging weight including maximum underpressure + burr weight + fire consumption.

[0054] The burr weight = the total weight of the warehouse filled 1 / 2 to completely filled in each fire, and the fire consumption in each fire is calculated as 0.05% to 2% of the weight of the blank.

[0055] In step S2, during die forging, burrs are likely to occur due to the thick burrs, and the burrs generally need to be polished and removed, otherwise they are easily pressed into the body during production; therefore, a width of 5 to 15 mm is reserved in the design of the female die of the die forging trimming die.

[0056] In step K3, the trimming is performed by a punch, and the punch includes a cylindrical end with a half-enclosed structure, which reduces the exposed area of ​​the forging and concentrates the shearing area, thereby preventing the generation of burrs.

[0057] By completely removing the burrs in the areas where the cavity is easy to fill, the tonnage required for forming is reduced; by retaining the burrs in the areas where the cavity is difficult to fill, the metal is prevented from flowing outward, which is conducive to filling the cavity with the blank; by completing the above-mentioned burr removal in a zoned manner while the forging is hot, continuous production of forgings can be achieved, saving energy and cycle time.

[0058] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A forging method for continuous die forging of a boss forging, characterized in that: The following steps are involved:

1. Design S1. Through blank design, die design and numerical simulation, find out the places where the forging is not filled during the forming process; S2, performing matching design of die forging 1 fire trimming die, in which the female die of die forging 1 fire trimming die is designed, the forging is positioned in the female die through the positioning position to perform positioning trimming, and the burrs are cut off; S3, after die forging 1 fire, the forgings are directly returned to the furnace; 2. Forging K1. Spray the manufactured blank evenly with alloy steel glass protective lubricant, and then heat it in a natural gas furnace at a heating temperature of 1150-1180°C and a heating coefficient of 0.3-0.6; K2, die forging 1 fire: die preheating temperature 350 ℃, preheating time ≥ 12 hours, put the heated blank into the cavity, straighten and level it, hit it lightly 1-2 times, lift the forging to blow off the oxide scale and then hit it hard to form, control the underpressure 10-20mm, and control the final forging temperature ≥ 850 ℃; K3. Transfer the forging to the die forging 1 fire trimming die for trimming, and the trimming temperature is ≥800℃; K4. Return the hot forgings after trimming to the furnace for heating at a temperature of 1150-1180°C and a heating coefficient of 0.15-0.4; K5, Die forging 2 fires: Still use the die forging 1 fire, the cavity temperature ≥ 200℃. Put the heated billet into the cavity, straighten and level it, hit it lightly 1-2 times, lift the forging to blow off the oxide scale and then hit it hard to form, control the underpressure to meet the requirements of the drawing, and control the final forging temperature ≥ 850℃; K6. Transfer the forging to the die forging 2-fire trimming die for trimming. The trimming temperature is ≥800℃. After trimming, the forging is corrected.

2. A design method for continuous die forging of a boss forging as claimed in claim 1, characterized in that: In step S1, the mold design includes a side bridge portion having a thickness of 4 to 8 mm and a width of 12 to 20 mm, and a rough edge bin portion having a thickness of 15 to 30 mm and a width of 50 to 80 mm.

3. A design method for continuous die forging of a boss forging as claimed in claim 2, characterized in that: The die is made of 5CrMnMo material. The die is used to forge the forgings by a 10-ton die forging hammer. The heating temperature of the forging blank is 1150-1180° C. The hot forging digital die is designed and manufactured according to the forging shrinkage rate of 1.5%.

4. The design method for continuous die forging of a boss forging according to claim 1, characterized in that: In step S1, the blank is designed according to the forging shape, and the burr weight and fire consumption are added by calculating the weight.

5. The design method for continuous die forging of a boss forging according to claim 1, characterized in that: In step S2, a width of 5 to 15 mm is reserved in the design of the female die of the die forging 1 fire trimming die.

6. The design method for continuous die forging of a boss forging according to claim 1, characterized in that: In step K3, the trimming is performed by a punch, and the punch includes a cylindrical end head with a half-enclosed structure.

Citation Information

Patent Citations

  • Precision forging process for twisting connector part of automotive chassis suspension system

    CN103100625A

  • Novel closed type blank discharging technology of thin-wall tendon deep upper opening narrow part

    CN103433412A

  • Forging method for complex thin-rib stainless steel die forging with center hole

    CN105215629A

  • Short-process forging method for super-large titanium alloy frame

    CN106040930A

  • Hot-working forging design method for ultrahigh-strength steel AerMet100

    CN112775372A