Method for improving quality of ultra-low carbon steel head blank
By removing the air in the middle of the pack before continuous casting and pouring, using alkaline and carbonized rice husk covering agent, optimizing the pouring speed curve and covering agent addition time, dynamically adjusting the oxygen detection frequency, ultra-low carbon steel head billet steel water is solved The problem of poor cleanliness significantly improves the quality and material yield of the head blank.
Patent Information
- Application Number
- CN202410996533.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
AI Technical Summary
The cleanliness of the ultra-low carbon steel head billets are poor, resulting in serious slag rolls and the quality of the normal cast billets is not achieved, resulting in waste of materials.
Before continuous casting and pouring, use an argon blowing tube to remove the air in the middle, measure the oxygen content and add alkaline and carbonized rice husk covering agent, optimize the pouring speed curve and the covering agent addition time, control the oxygen content and inclusion floating, Dynamically adjust the detection frequency through an oxygen detector.
Effectively prevent air pollution of the molten steel, reduce the amount of exposed molten steel, adsorb inclusions, control the inclusion of slag on the head, and improve the quality and material yield of the head blank.
Smart Images

Figure CN118905169A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steelmaking and continuous casting, and in particular to a method for improving the quality of ultra-low carbon steel head billet. Background Art
[0002] The head slab refers to the first slab cast in the continuous casting process. Due to the direct contact of molten steel with air during pouring, the molten steel is oxidized, and the oxygen and nitrogen content in the head slab is abnormally high. At the same time, the liquid level in the flow field of the crystallizer fluctuates greatly during pouring, which can easily cause slag rolling, resulting in poor cleanliness of the molten steel in the head slab and serious slag rolling, which cannot reach the quality of normal castings. The head slab can only be downgraded or scrapped, resulting in serious waste of materials. Therefore, it is necessary to develop new technologies to improve the quality of ultra-low carbon steel head slabs.
[0003] At present, the existing process technology to improve the quality of the head billet mainly relies on the use of argon blowing to remove the air in the tundish before pouring, but the quality improvement of the head billet is limited and the qualified rate is still low. Therefore, inventing a method that can stably improve the quality of ultra-low carbon steel head billets is of great significance to improving the yield rate. Summary of the invention
[0004] The purpose of the present invention is to provide a method for improving the quality of ultra-low carbon steel head billets, so as to solve the problem that the ultra-low carbon steel head billets in the prior art have poor cleanliness of molten steel and cannot reach the quality of normal billets.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A method for improving the quality of ultra-low carbon steel head blanks comprises the following steps:
[0007] Step 1: Before continuous casting, use an argon blowing tube to blow argon into the tundish, and use an oxygen meter to measure the oxygen content in the tundish until the oxygen content in the tundish is less than 1%, then stop blowing argon;
[0008] Step 2: When continuous casting starts, when the molten steel tonnage in the continuous casting tundish reaches 10 tons, first add the lower layer of alkaline covering agent, add 4-5 bags to each hole, and then add the heat-insulating carbonized rice husk covering agent until the surface of the molten steel in the tundish is all black slag;
[0009] Step 3: During the continuous casting process, when the tonnage of the tundish reaches more than 25 tons, the tundish stopper rod is opened to start pouring in the crystallizer;
[0010] Step 4: During the continuous casting process, after starting the crystallizer casting, the starting casting speed is set to 0.3 m / min and maintained for 20 seconds; then the casting speed is directly increased to 1.0 m / min at an acceleration of 0.2 m / S, and then evenly increased to 1.5 m / min;
[0011] Step 5: Cut the head of the continuous casting head billet while maintaining a pulling speed of 1.5 m / min.
[0012] As a further solution of the present invention: during the measurement of the oxygen content in the bag using an oxygen meter, the detection frequency is increased as the oxygen content decreases.
[0013] As a further solution of the present invention: when the oxygen content is ≥10%, the oxygen meter detects once every three minutes; when 10%>oxygen content ≥5%, it detects once every two minutes; when 5%>oxygen content ≥1%, it detects once every minute; when the oxygen content is <1%, argon blowing is stopped.
[0014] As a further solution of the present invention: the cut length of the continuous casting head billet is 2-2.1 meters.
[0015] Beneficial effects of the present invention:
[0016] (1) Use an oxygen meter to measure the oxygen content in the tundish when pouring begins. Stop blowing argon when the oxygen content in the tundish is less than 1%. This can effectively prevent air from contaminating the molten steel.
[0017] (2) Rapid double-layer covering can reduce the amount of exposed molten steel at the beginning of pouring as early as possible. The lower layer of alkaline covering agent can also quickly absorb the inclusions floating up from the molten steel, further improving the cleanliness of the molten steel at the beginning of pouring.
[0018] (3) Optimizing the time of adding the covering agent and optimizing the tonnage of the tundish can reduce the amount of exposed molten steel at the time of pouring as early as possible, promote the floating of inclusions in the molten steel, and further improve the cleanliness of the molten steel at the time of pouring.
[0019] (4) Optimizing the pouring speed curve can effectively control the inclusion of slag within 2 meters of the head. The ultra-low carbon steel head is controlled to be about 2 meters, which can just cut off the exposed part of the molten steel in the middle package, so that the quality of the head billet can be effectively improved, so the present invention has a high value of promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The present invention will be further described below in conjunction with the accompanying drawings.
[0021] Figure 1 is a flow chart of the method of the present invention. DETAILED DESCRIPTION
[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] See also Figure 1 As shown, the present invention is a method for improving the quality of ultra-low carbon steel head billet, comprising the following steps:
[0024] Step 1: Before continuous casting starts, use an argon blowing tube to blow argon into the tundish, and use an oxygen meter to measure the oxygen content in the tundish until the oxygen content in the tundish is less than 1%, then stop blowing argon; use an oxygen meter to measure the oxygen content in the tundish when casting starts, and stop blowing argon when the oxygen content in the tundish is less than 1%, which can effectively prevent air from contaminating the molten steel.
[0025] Step 2, when continuous casting starts, when the molten steel tonnage of the continuous casting tundish reaches 10 tons, first add the lower layer of alkaline covering agent, add 4-5 bags to each hole, and then add the heat-insulating carbonized rice husk covering agent until the surface of the molten steel in the tundish is covered with black slag; rapid double-layer covering can reduce the amount of exposed molten steel as soon as possible when pouring starts, and the lower layer of alkaline covering agent can also quickly absorb the inclusions floating from the molten steel, optimize the covering agent addition time and optimize the tundish pouring tonnage, so as to reduce the amount of exposed molten steel as soon as possible when pouring starts, and promote the floating inclusions in the molten steel, further improve the cleanliness of the molten steel when pouring starts.
[0026] Step 3: During the continuous casting process, when the tonnage of the tundish reaches more than 25 tons, the tundish stopper rod is opened to start pouring in the crystallizer. This increases the floating time of inclusions in the molten steel in the tundish and makes the molten steel cleaner.
[0027] Step 4: During the continuous casting process, after the crystallizer is started, the starting speed is set to 0.3m / min and maintained for 20s; then the speed is directly increased to 1.0m / min at an acceleration of 0.2m / S, and then evenly increased to 1.5m / min; the length of the continuous casting head billet is 2-2.1 meters, and the pouring speed increase curve is optimized to effectively control the slag inclusion within 2 meters of the head. The ultra-low carbon steel head is controlled at about 2 meters, which can just cut off the exposed part of the molten steel in the middle package, which can effectively improve the quality of the head billet, so the present invention has a high value of promotion and application.
[0028] Step 5: Cut the continuous casting head billet while maintaining a pulling speed of 1.5 m / min.
[0029] When using an oxygen meter to measure the oxygen content in the package, increase the detection frequency as the oxygen content decreases.
[0030] When the oxygen content is ≥10%, the oxygen meter detects once every three minutes; when 10%>oxygen content ≥5%, it detects once every two minutes; when 5%>oxygen content ≥1%, it detects once every minute; when the oxygen content is <1%, stop blowing argon.
[0031] Specifically, changing the measurement frequency according to the oxygen content can, on the one hand, reduce unnecessary measurements in the early stages, thereby reducing workload; on the other hand, increasing the measurement frequency when the oxygen content decreases can effectively ensure that the oxygen content is within the required optimal range, thereby avoiding the impact of too little oxygen content on production quality due to reduced measurement frequency.
[0032] The working principle of the present invention: Taking the casting of ultra-low carbon steel as an example, the number of continuous casting furnaces is 10, the continuous casting speed is 1.5m / min, and the specifications of the continuous casting billet are: 240mm×1120mm, which is a one-machine two-stream continuous casting machine. Before the continuous casting starts, the argon blowing tube is used to blow argon into the middle ladle. After three minutes, the oxygen content in the middle ladle is measured using an oxygen meter until the argon blowing is stopped when the oxygen content in the middle ladle is less than 1%. When pouring, when the molten steel tonnage of the continuous casting middle ladle reaches 10 tons, the lower layer of alkaline covering agent is added first, and after adding 4-5 bags to each hole, the heat-insulating carbonized rice husk covering agent is quickly added until the surface of the molten steel in the middle ladle is all black slag. When the tonnage of the middle ladle is more than 25 tons, the middle ladle plug rod is opened to start pouring in the crystallizer. After starting the crystallizer to draw the billet, the starting drawing speed is set to 0.3m / min and maintained for 20s; then the acceleration is directly increased to 1.0m / min at 0.2m / S2, and then quickly increased to 1.5m / min. The head cutting is operated at 2.0m. According to the hot rolling quality tracking, the quality of the first billet of this casting is normal, without any reduction, modification or scrapping.
[0033] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.
Claims
1. A method for improving the quality of ultra-low carbon steel head billet, It is characterized in that The following steps are involved: Step 1: Before continuous casting, use an argon blowing tube to blow argon into the tundish, and use an oxygen meter to measure the oxygen content in the tundish until the oxygen content in the tundish is less than 1%, then stop blowing argon; Step 2: When continuous casting starts, when the molten steel tonnage in the continuous casting tundish reaches 10 tons, first add the lower layer of alkaline covering agent, add 4-5 bags to each hole, and then add the heat-insulating carbonized rice husk covering agent until the surface of the molten steel in the tundish is all black slag; Step 3: During the continuous casting process, when the tonnage of the tundish reaches more than 25 tons, the tundish stopper rod is opened to start pouring in the crystallizer; Step 4: During the continuous casting process, after starting the crystallizer casting, the starting casting speed is set to 0.3 m / min and maintained for 20 seconds; then the casting speed is directly increased to 1.0 m / min at an acceleration of 0.2 m / S, and then evenly increased to 1.5 m / min; Step 5: Cut the continuous casting head billet while maintaining a pulling speed of 1.5 m / min.
2. A method for improving the quality of ultra-low carbon steel head billet according to claim 1, It is characterized in that When using an oxygen meter to measure the oxygen content in the package, increase the detection frequency as the oxygen content decreases.
3. A method for improving the quality of ultra-low carbon steel head billet according to claim 2, It is characterized in that When the oxygen content is ≥10%, the oxygen meter detects once every three minutes; when 10%>oxygen content ≥5%, it detects once every two minutes; when 5%>oxygen content ≥1%, it detects once every minute; when the oxygen content is <1%, stop blowing argon.
4. A method for improving the quality of ultra-low carbon steel head billet according to claim 1, It is characterized in that The length of the continuous casting head billet is 2-2.1 meters.