Target material welding method and obtained welding target material

By setting a detachable barrier strip around the back plate boss to form a solder layer, the cracking problem caused by bending deformation of the brittle target during sputtering coating is solved, effective buffering of the target stress is achieved, and the coating process is improved Stability and efficiency.

CN118905488APending Publication Date: 2024-11-08KONFOONG MATERIALS INTERNATIONAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411256678.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

During the sputtering coating process, brittle targets are prone to cracking due to external stress, which affects the continuity and uniformity of the film. The existing methods of increasing the thickness of the solder layer cannot effectively buffer the stress of bending deformation.

Method used

Detachable barrier strips are arranged around the boss of the back plate to form a storage space to fill solder. After preheating, the welding surface of the target material is placed on the surface of the solder layer for welding, and the barrier strip is removed after cooling to realize the production of the welding target material. , avoid using hard substances to assist.

Benefits of technology

By adjusting the thickness of the solder layer, the bending and deformation stress of the target material can be effectively buffered, the reliability and efficiency of the sputtering coating process can be improved, and cracking will be avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905488A_ABST
    Figure CN118905488A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of welding, and provides a target material welding method and an obtained welding target material, the welding method comprises the steps that barrier strips are arranged on the periphery of a boss of a back plate, a containing space is formed by the barrier strips and the horizontal surface of the boss, and welding flux is filled to form a welding flux layer; the welding face of the preheated target blank is placed on the surface of the welding flux layer, and welding is started; and after welding is finished, cooling is conducted, the barrier strips are detached, and the welding target material is obtained. According to the welding method, assistance of hard substances such as a cylindrical boss and a copper wire is not used, the thickness of the welding flux layer can be adjusted and controlled according to needs, welding is achieved, and therefore the thickness of the welding flux layer is effectively utilized to achieve buffering of deformation such as target material bending or deformation acting force.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of welding, and relates to a welding method of a target material and the obtained welding target material. Background Art

[0002] With the continuous development of integrated circuit technology, thin film deposition process occupies an extremely important position in the manufacture of semiconductor devices. Among them, physical vapor deposition (PVD) technology has been widely used in the semiconductor industry due to its simple process, fast deposition rate, and good film uniformity. Sputtering coating, as a main method of PVD, is mainly used to prepare metal films, insulating films and other functional films. However, in the sputtering coating process, the selection and design of the target material are directly related to the quality of the film and the stability of the deposition process. Especially for targets made of certain brittle materials, problems such as cracking are prone to occur during use, which affects the continuity and uniformity of the film.

[0003] Specifically, brittle targets, such as targets containing silicon (WSi, CrSi or Si, etc.) or Ge targets, have higher hardness and lower ductility due to their own material properties. This brittle characteristic makes these targets more likely to break rather than plastically deform when subjected to external stress. During the sputtering coating process, the target is usually fixed on a backing plate and placed in a vacuum environment to receive ion bombardment. At this time, due to factors such as the negative pressure generated by the sputtering action, water pressure, and the pressure of the cooling water on the back of the target, the target may experience varying degrees of bending deformation. For brittle targets, this deformation can easily cause stress concentration inside the material, resulting in cracking of the target, affecting the quality and deposition efficiency of the sputtered film.

[0004] In order to solve the problem of cracking that may occur during the use of brittle targets, researchers have proposed a series of improvement measures. Among them, increasing the thickness of the solder layer between the target and the back plate is considered to be an effective mitigation method. As a connecting medium between the target and the back plate, the main function of the solder layer is to provide sufficient mechanical support and good thermal conductivity. In theory, thickening the solder layer can act as a buffer, reducing the stress on the target when it is bent and deformed, thereby avoiding the occurrence of cracking.

[0005] At present, there are two common specific implementation plans: one is to design a small cylindrical boss on the back plate; the other is to place copper wire during the welding process. The purpose of these two methods is to increase the average thickness of the entire solder layer by increasing the local thickness of the solder layer. However, both methods have obvious defects. First, although the design of the small cylindrical boss can achieve local thickening, due to its fixed structure, it cannot deform freely with the bending of the target material, and therefore cannot really play a buffering role. Secondly, although the method of placing copper wire can increase the thickness of the solder layer to a certain extent, due to the strong rigidity of the copper wire itself, it is also unable to effectively disperse stress. Therefore, although these two methods can theoretically increase the thickness of the solder layer, they cannot play a practical buffering role, making it meaningless to increase the solder thickness.

[0006] Therefore, it is necessary to develop a more scientific and reasonable welding scheme so that the increase in the thickness of the solder layer can play a practical effect and role, thereby improving the reliability and efficiency of the sputtering coating process. Summary of the invention

[0007] In view of the problems existing in the prior art, the purpose of the present invention is to provide a welding method for a target material and a welding target material obtained, wherein the welding method includes setting a baffle around the boss of the back plate to form a containing space with the horizontal surface of the boss to fill the solder to form a solder layer; placing the welding surface of the preheated target blank on the surface of the solder layer to start welding; after the welding is completed, cooling is performed, and the baffle is removed to obtain a welding target material. The welding method of the present invention does not use the assistance of hard materials such as cylindrical bosses and copper wires, and can adjust and control the thickness of the solder layer as needed to achieve welding, thereby effectively utilizing the thickness of the solder layer to achieve the buffering of deformation or deformation force such as bending of the target material.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a target material welding method, the target material welding method comprising:

[0010] (1) providing a target blank to be welded and a backing plate; a boss is arranged on the backing plate, and baffles are detachably arranged around the boss, and the height of the baffles is higher than the horizontal surface of the boss to form a receiving space; the receiving space is filled with solder to form a solder layer;

[0011] (2) after preheating the target blank and the back plate to the welding temperature, placing the welding surface of the preheated target blank on the surface of the solder layer in the accommodation space to start welding;

[0012] (3) After welding, the welding target is cooled and the baffle is removed to obtain the welding target.

[0013] The welding method described in the present invention does not use hard materials such as cylindrical bosses and copper wires in the prior art to assist in the solder layer, but uses baffles arranged around the bosses to form a space for accommodating the solder, so that the solder can form a pure solder layer that fills and paves the surface of the bosses, and further controls the surface contact between the welding surface of the target blank and the solder layer, so that the welding process can be successfully completed. The solder layer after welding is uniform as a whole without the obstruction of other hard materials. Therefore, the thickness of the solder layer can be adjusted and controlled as needed, and the thickness of the solder layer can also be used to effectively achieve buffering of deformation or deformation force such as bending of the target material.

[0014] The following are preferred technical solutions of the present invention, but are not intended to be limitations of the technical solutions provided by the present invention. Through the following technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.

[0015] As a preferred technical solution of the present invention, in step (1), the target blank includes a brittle target blank.

[0016] As a preferred technical solution of the present invention, the material of the brittle target blank includes at least one of WSi, CrSi, Si or Ge.

[0017] As a preferred technical solution of the present invention, the solder includes In solder or 919 solder.

[0018] As a preferred technical solution of the present invention, the welding temperature of the In solder is 180-240°C, for example, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C or 240°C, and the welding temperature of the 919 solder is 200-280°C, for example, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, 260°C, 270°C or 280°C, but is not limited to the listed values, and other unlisted values ​​within the above numerical range are also applicable.

[0019] As a preferred technical solution of the present invention, in step (1), the shape of the horizontal surface of the boss is the same as the shape of the target blank.

[0020] As a preferred technical solution of the present invention, in step (1), the size of the horizontal surface of the boss is the same as the size of the target blank.

[0021] As a preferred technical solution of the present invention, in step (1), the accommodating space does not contain any hard material except the solder; the hard material includes a cylindrical boss and / or a copper wire.

[0022] As a preferred technical solution of the present invention, the diameter of the cylindrical boss is 1 to 10 mm, for example, 1 mm, 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm or 10 mm, and the height is 1 to 3 mm, for example, 1 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm, 1.5 mm, 1.6 mm, 1.7 mm, 1.8 mm, 1.9 mm, 2 mm, 2.1 mm, 2.2 mm, 2.3 mm, 2.4 mm, 2.5 mm, 2.6 mm, 2.7 mm, 2.8 mm, 2.9 mm or 3 mm, but is not limited to the listed values, and other values ​​not listed within the above numerical range are also applicable.

[0023] As a preferred technical solution of the present invention, in step (1), the height difference between the baffle and the horizontal surface of the boss is the thickness of the solder layer; the thickness of the solder layer is 1 to 3 mm, for example, 1 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm, 1.5 mm, 1.6 mm, 1.7 mm, 1.8 mm, 1.9 mm, 2 mm, 2.1 mm, 2.2 mm, 2.3 mm, 2.4 mm, 2.5 mm, 2.6 mm, 2.7 mm, 2.8 mm, 2.9 mm or 3 mm, but is not limited to the listed values, and other values ​​not listed within the above numerical range are equally applicable.

[0024] In the present invention, the height difference between the baffle and the horizontal surface of the boss, that is, the thickness of the solder layer should be reasonably selected and adjusted. If the solder layer thickness is too small, it cannot effectively buffer the bending of the target blank. When it has a suitable buffering effect, an excessively thick solder layer cannot further enhance the buffering effect, causing waste and increasing costs.

[0025] As a preferred technical solution of the present invention, in step (1), the baffle comprises a stainless steel thin strip.

[0026] As a preferred technical solution of the present invention, in step (2), after the target blank and the back plate are preheated to the welding temperature, the welding surface of the preheated target blank is pre-wetted with solder and then placed on the surface of the solder layer in the accommodating space to start the welding.

[0027] As a preferred technical solution of the present invention, in step (2), the welding surface of the preheated target blank is placed on the surface of the solder layer in the accommodating space by hoisting.

[0028] In the present invention, when the welding surface of the target blank is slowly placed on the surface of the solder layer on the back plate by hoisting, it is visually confirmed that the entire welding surface of the target blank is in contact with the solder layer and maintains contact to complete the welding process.

[0029] As a preferred technical solution of the present invention, the hoisting method includes using a hoisting rod provided with a suction cup to adsorb the suction cup to the other side surface of the target blank opposite to the welding surface for hoisting.

[0030] As a preferred technical solution of the present invention, in step (3), when the cooling is performed until the temperature drops to half the melting temperature of the solder, the baffle and the suction cup are removed.

[0031] As a preferred technical solution of the present invention, in step (3), the cooling is natural cooling in the air.

[0032] In a second aspect, the present invention provides a welding target material obtained according to the welding method described in the first aspect.

[0033] Compared with the prior art solutions, the present invention has at least the following beneficial effects:

[0034] The welding method described in the present invention does not use hard materials such as cylindrical bosses and copper wires in the prior art to assist in the solder layer, but uses baffles arranged around the bosses to form a space for accommodating the solder, so that the solder can form a pure solder layer that fills and paves the surface of the bosses, and further controls the surface contact between the welding surface of the target blank and the solder layer, so that the welding process can be successfully completed. The solder layer after welding is uniform as a whole without the obstruction of other hard materials. Therefore, the thickness of the solder layer can be adjusted and controlled as needed, and the thickness of the solder layer can also be used to effectively achieve buffering of deformation or deformation force such as bending of the target material. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 is a schematic flow chart of the target material welding method in Example 1;

[0036] In the figure: 1-back plate, 2-boss, 3-block bar, 4-solder layer, 5-target blank, 6-suspender rod, 7-suction cup. DETAILED DESCRIPTION

[0037] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0038] It should be clear to those skilled in the art that the embodiments are only intended to help understand the present invention and should not be considered as specific limitations of the present invention.

[0039] In some specific embodiments, the present invention provides a target material welding method, the target material welding method comprising:

[0040] (1) providing a target blank to be welded and a backing plate; a boss is arranged on the backing plate, and baffles are detachably arranged around the boss, and the height of the baffles is higher than the horizontal surface of the boss to form a receiving space; the receiving space is filled with solder to form a solder layer;

[0041] (2) after preheating the target blank and the back plate to the welding temperature, placing the welding surface of the preheated target blank on the surface of the solder layer in the accommodation space to start welding;

[0042] (3) After welding, the welding target is cooled and the baffle is removed to obtain the welding target.

[0043] In one embodiment, in step (1), the target blank includes a brittle target blank.

[0044] In one embodiment, the material of the brittle target blank includes at least one of WSi, CrSi, Si or Ge.

[0045] In one embodiment, the solder includes In solder or 919 solder.

[0046] In one embodiment, the soldering temperature of the In solder is 180-240°C.

[0047] In one embodiment, the soldering temperature of the 919 solder is 200-280°C.

[0048] In one embodiment, in step (1), the shape of the horizontal surface of the boss is the same as the shape of the target blank.

[0049] In one embodiment, in step (1), the size of the horizontal surface of the boss is the same as the size of the target blank.

[0050] In one embodiment, in step (1), the accommodating space does not contain any hard material except the solder; the hard material includes a cylindrical boss and / or a copper wire.

[0051] In one embodiment, the cylindrical boss has a diameter of 1 to 10 mm and a height of 1 to 3 mm.

[0052] In one embodiment, in step (1), the height difference between the baffle and the horizontal surface of the boss is the thickness of the solder layer; the thickness of the solder layer is 1 to 3 mm.

[0053] In one embodiment, in step (1), the barrier strip comprises a stainless steel strip.

[0054] In one embodiment, in step (2), after the target blank and the back plate are preheated to the welding temperature, the welding surface of the preheated target blank is pre-wetted with solder and then placed on the surface of the solder layer in the accommodating space to start the welding.

[0055] In one embodiment, in step (2), the welding surface of the preheated target blank is placed on the surface of the solder layer in the accommodation space by hoisting.

[0056] In one embodiment, the hoisting method includes using a hoisting rod provided with a suction cup to adsorb the suction cup onto another side surface of the target blank opposite to the welding surface for hoisting.

[0057] In one embodiment, in step (3), the blocking bar and the suction cup are removed when the cooling is performed until the temperature drops to half the melting temperature of the solder.

[0058] In one embodiment, in step (3), the cooling is natural cooling in air.

[0059] In some specific embodiments, the present invention provides a welding target material obtained according to the welding method provided in the above embodiments.

[0060] Example 1

[0061] This embodiment provides a target material welding method, such as Figure 1 As shown, the welding method comprises:

[0062] (1) providing a target blank 5 and a backing plate 1 to be welded; the target blank 5 is a WSi target with a diameter of 200 nm; a boss 2 is arranged on the backing plate 1, and the shape and size of the horizontal surface of the boss 2 are the same as those of the target blank 5; a baffle 3 is detachably arranged around the boss 2, and the height of the baffle 3 is higher than the horizontal surface of the boss 2 to form a receiving space; the baffle 3 is a stainless steel thin strip; the receiving space is filled with solder (In solder), and except for the solder, no hard materials such as the cylindrical boss 2 and / or copper wire are contained, and the solder forms a solder layer 4; the height difference between the baffle 3 and the horizontal surface of the boss 2 is the thickness of the solder layer 4, and the thickness of the solder layer 4 is 2 mm;

[0063] (2) After the target blank 5 and the back plate 1 are preheated to a welding temperature of 180 to 240° C., a suspension rod 6 provided with a suction cup 7 is used to adsorb the suction cup 7 to the other side of the target blank 5 opposite to the welding surface, and the target blank 5 is hoisted, and the welding surface of the preheated target blank 5 in the hoisted target blank 5 is controlled to be infiltrated with solder, and then the welding surface infiltrated with solder is continuously hoisted on the surface of the solder layer 4 in the accommodating space to start welding;

[0064] (3) After welding, the target is naturally cooled in the air. When the temperature drops to half of the melting temperature of the solder, the baffle 3 and the suction cup 7 are removed to obtain a welding target.

[0065] Example 2

[0066] This embodiment provides a target material welding method, the welding method comprising:

[0067] (1) providing a target blank and a backing plate to be welded; the target blank is a CrSi target with a diameter of 200 nm; a boss is arranged on the backing plate, and the shape and size of the horizontal surface of the boss are the same as those of the target blank; the boss is detachably surrounded by a baffle, and the height of the baffle is higher than the horizontal surface of the boss to form a receiving space; the baffle is a stainless steel strip; the receiving space is filled with solder (In solder), and except for the solder, no hard substances such as cylindrical bosses and / or copper wires are contained, and the solder forms a solder layer; the height difference between the baffle and the horizontal surface of the boss is the thickness of the solder layer, and the thickness of the solder layer is 2 mm;

[0068] (2) After the target blank and the back plate are preheated to a welding temperature of 180 to 240° C., a suspension rod provided with a suction cup is used to adsorb the suction cup to the other side of the target blank opposite to the welding surface, and the target blank is hoisted, and the welding surface of the preheated target blank in the hoisted target blank is controlled to be infiltrated with solder, and then the welding surface infiltrated with solder is continuously hoisted on the surface of the solder layer in the accommodating space to start welding;

[0069] (3) After welding, the target is naturally cooled in the air. When the temperature drops to half of the melting temperature of the solder, the baffle and the suction cup are removed. The baffle is removed to obtain a welding target.

[0070] Example 3

[0071] This embodiment provides a target material welding method, the welding method comprising:

[0072] (1) providing a target blank and a backing plate to be welded; the target blank is a Ge target with a diameter of 200 mm; a boss is arranged on the backing plate, and the shape and size of the horizontal surface of the boss are the same as those of the target blank; the boss is detachably surrounded by baffles, and the height of the baffles is higher than the horizontal surface of the boss to form a receiving space; the baffles are stainless steel strips; the receiving space is filled with solder (In solder), and except for the solder, no hard substances such as cylindrical bosses and / or copper wires are contained, and the solder forms a solder layer; the height difference between the baffles and the horizontal surface of the boss is the thickness of the solder layer, and the thickness of the solder layer is 2 mm;

[0073] (2) After the target blank and the back plate are preheated to a welding temperature of 180 to 240° C., a suspension rod provided with a suction cup is used to adsorb the suction cup to the other side of the target blank opposite to the welding surface, and the target blank is hoisted, and the welding surface of the preheated target blank in the hoisted target blank is controlled to be infiltrated with solder, and then the welding surface infiltrated with solder is continuously hoisted on the surface of the solder layer in the accommodating space to start welding;

[0074] (3) After welding, the target is naturally cooled in the air. When the temperature drops to half of the melting temperature of the solder, the baffle and the suction cup are removed. The baffle is removed to obtain a welding target.

[0075] Example 4

[0076] This embodiment provides a method for welding a target material. In step (1) of the welding method, the height difference between the baffle and the horizontal surface of the boss is adjusted, that is, the thickness of the solder layer is adjusted from 1 mm to 0.5 mm. Except for the above, other conditions are exactly the same as those in Example 1.

[0077] Example 5

[0078] This embodiment provides a method for welding a target material. In step (1) of the welding method, the height difference between the baffle and the horizontal surface of the boss is adjusted, that is, the thickness of the solder layer is adjusted from 1 mm to 3 mm. Except for the above, other conditions are exactly the same as those in Example 1.

[0079] Example 6

[0080] This embodiment provides a method for welding a target material. In step (1) of the welding method, the height difference between the baffle and the horizontal surface of the boss is adjusted, that is, the thickness of the solder layer is adjusted from 1 mm to 4 mm. Except for the above, other conditions are exactly the same as those in Example 1.

[0081] Comparative Example 1

[0082] This comparative example provides a target material welding method, the welding method comprising:

[0083] A target blank and a back plate to be welded are provided; the target blank is a WSi target with a diameter of 200 nm; four small cylindrical bosses with a diameter of 6 mm and a height of 3 mm are welded in advance on the welding surface of the back plate; the target blank is placed on the small cylindrical bosses, and the target blank is supported by the small cylindrical bosses, so that a solder thickness of 2 mm is left between the target blank and the back plate during welding, the solder is In solder, and the welding temperature is controlled to be 180-240°C.

[0084] Comparative Example 2

[0085] This comparative example provides a target material welding method, the welding method comprising:

[0086] A target blank and a back plate to be welded are provided; the target blank is a WSi target with a diameter of 200 nm; solder is first placed on the welding surface of the back plate for stacking, and then a copper wire is placed, and then the target blank is placed on the copper wire, and the target blank is supported by the copper wire, so that a solder thickness of 2 mm is left between the target blank and the back plate during welding, the solder is In solder, and the welding temperature is controlled to be 180-240°C.

[0087] Characterization and Testing:

[0088] The welding target materials obtained in the embodiment and the comparative example were tested. The target blank side of the finished target material was placed on the pad with the pad facing downward, and the pad was also placed in the back plate area. The hydraulic press head was aligned with the core of the target material, and pressure was applied to 5t (try to ensure that the curvature of the back plate is 4mm±0.1mm). After pressurization, the target material was taken down and the curvature of the sputtering surface and the curvature of the back plate of the target material were detected with a test fixture, and the target blank was checked for cracks. The results are recorded in Table 1.

[0089] Table 1

[0090] Group Back panel curvature (mm) Target curvature (mm) Example 1 4.05 0.45 not cracked Example 2 4.10 0.58 Not cracked Example 3 4.00 0.55 not cracked Example 4 4.05 2.84 Cracking Example 5 4.10 0.40 Not cracked Example 6 4.05 0.37 Not cracked Comparative Example 1 3.95 2.35 Cracking Comparative Example 2 4.00 2.24 Cracking

[0091] It can be seen from Table 1 that:

[0092] The target materials of various materials in Examples 1 to 3 can prevent the target blank from cracking by using the welding method of the present invention. By comparing Example 1 with Examples 4-6, it is found that the thicker the solder layer, the better the welding effect of the solder layer. By comparing Example 1 with Comparative Examples 1-2, it is found that the welding method of the comparative example has a very limited buffering effect on the target blank, while the welding method of the present invention has a very obvious buffering effect on the target blank.

[0093] From the above, it can be seen that the welding method described in the present invention does not use the cylindrical bosses, copper wires and other hard materials in the prior art to assist in the solder layer, but uses baffles arranged around the bosses to form a space to accommodate the solder, so that the solder can form a pure solder layer that fills and paves the surface of the bosses, and further control the contact between the welding surface of the target blank and the surface of the solder layer, so that the welding process can be successfully completed. The solder layer after welding is uniform as a whole without the obstruction of other hard materials. Therefore, the thickness of the solder layer can be adjusted and controlled as needed, and the thickness of the solder layer can also be used to effectively achieve the buffering of deformation or deformation force such as bending of the target material.

[0094] The present invention illustrates the detailed process equipment and process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process equipment and process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process equipment and process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0095] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0096] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0097] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A target welding method, characterized in that: The welding method comprises: (1) providing a target blank to be welded and a backing plate; a boss is arranged on the backing plate, and baffles are detachably arranged around the boss, and the height of the baffles is higher than the horizontal surface of the boss to form a receiving space; the receiving space is filled with solder to form a solder layer; (2) after preheating the target blank and the back plate to the welding temperature, placing the welding surface of the preheated target blank on the surface of the solder layer in the accommodation space to start welding; (3) After welding, the welding target is cooled and the baffle is removed to obtain the welding target.

2. The target welding method according to claim 1, characterized in that: In step (1), the target blank comprises a brittle target blank; Preferably, the material of the brittle target blank includes at least one of WSi, CrSi, Si or Ge.

3. The target welding method according to claim 1, characterized in that: In step (1), the shape of the horizontal surface of the boss is the same as the shape of the target blank; Preferably, the size of the horizontal surface of the boss is the same as that of the target blank.

4. The target welding method according to claim 1, characterized in that: The accommodation space in step (1) does not contain any hard material except the solder; the hard material includes a cylindrical boss and / or a copper wire.

5. The target welding method according to claim 1, characterized in that: In step (1), the height difference between the baffle and the horizontal surface of the boss is the thickness of the solder layer; The thickness of the solder layer is 1 to 3 mm.

6. The target welding method according to claim 1, characterized in that: In step (1), the baffle comprises a stainless steel thin strip.

7. The target welding method according to claim 1, characterized in that: In step (2), after the target blank and the back plate are preheated to the welding temperature, the welding surface of the preheated target blank is pre-wetted with solder and then placed on the surface of the solder layer in the accommodating space to start the welding.

8. The target welding method according to claim 1, characterized in that: In step (2), the welding surface of the preheated target blank is placed on the surface of the solder layer in the accommodating space by hoisting.

9. The target welding method according to claim 8, characterized in that: The hoisting method includes using a hoisting rod provided with a suction cup to adsorb the suction cup onto the other side surface of the target blank opposite to the welding surface for hoisting.

10. A welding target material, characterized in that: Obtained according to the welding method according to any one of claims 1 to 9.