Preparation method of electric contact gold alloy thick-wall thin pipe
Through multi-pass processing methods of hot forging, rotary forging, cold rolling, cold drawing and vacuum annealing, the problems of uneven structural performance and poor inner surface quality of the thick-walled thin tube of gold alloy are solved, and the thick-walled thin-walled thin-walled thin-walled thin-walled thin-walled thin-walled The uniform performance and efficient production of pipes meet the technical standards of precious metals and alloy pipes for conductive rings.
Patent Information
- Application Number
- CN202411173150.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-08
AI Technical Summary
The existing preparation methods for metal alloy thick-walled thin pipes lead to uneven tissue performance, low hardness, poor inner surface quality, and cracking problems, making it difficult to meet the technical standards of precious metals and alloy pipes for conductive rings.
Using multiple pass processing such as hot forging, rotary forging, cold rolling and cold drawing combined with vacuum annealing, microscopic defects are eliminated through hot forging, compressive stress deformation is controlled, cold rolling and cold drawing are uniformly deformed, and vacuum annealing is uniform. To ensure uniform finish and tissue performance of the inner and outer surfaces.
The finished product of thick-walled thin tubes has uniform structure performance, high inner surface finish and high production efficiency, meeting the technical standards of YS/T 207-2013 "Naught Metals for Conductive Rings and Its Alloy Pipes" and avoiding cracking and other defects.
Smart Images

Figure CN118905573A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal tube processing, and in particular relates to a method for preparing an electrical contact gold alloy thick-walled thin tube. Background Art
[0002] Gold alloy has high electrical and thermal conductivity, high chemical stability, low and stable contact resistance, high resistance to arc erosion and other properties. It is an irreplaceable excellent electrical contact material, ensuring the stable transmission of current and signals between two relatively rotating parts. Precious metal electrical contact alloys are used in various industrial fields such as aerospace, wind power generation, and security industry.
[0003] Gold alloys are used for small load electrical contact elements, mainly including AuAgCu, AuCuNi and other series alloys, which have good plastic processing properties and have been well applied as conductive ring materials, making the contact elements have a long service life, high working reliability and output accuracy. These alloys are plastically formed into thick-walled thin tubes, and then precisely machined into rings for the preparation of precision micro conductive slip rings.
[0004] The commonly used preparation method for thick-walled thin tubes is to bore the gold alloy ingot, anneal it multiple times and roll the tube, and then draw it to the finished size. The thick-walled thin tubes prepared by this method have uneven microstructure and properties, low hardness, many internal microscopic defects, poor inner surface quality, and wrinkle defects, which lead to cracking problems during the turning of conductive ring materials. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a method for preparing a thick-walled fine tube of an electrical contact gold alloy in view of the above-mentioned deficiencies of the prior art. The method for preparing a thick-walled fine tube of an electrical contact gold alloy of the present invention can effectively avoid defects such as uneven microstructure and mechanical cracking of the gold alloy thick-walled fine tube prepared by the prior art, and has the characteristics of uniform microstructure and performance of the finished product, high inner surface finish and high production efficiency, and meets the requirements of the technical standard YS / T 207-2013 "Precious metal and alloy tubes for conductive rings".
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a thick-walled thin tube of an electrical contact gold alloy, characterized in that it comprises:
[0007] Step 1, surface treating the cylindrical gold alloy ingot;
[0008] Step 2, hot forging the surface treated ingot to obtain a gold alloy bar blank;
[0009] Step 3, removing the shrinkage holes at both ends of the gold alloy rod blank, leveling and centering the hole, removing the surface oxide layer and folding by turning, and then drilling with a drill bit with an outer diameter of 9 to 14 mm to obtain a gold alloy tube blank;
[0010] Step 4: placing a charcoal box in a resistance furnace, heating the furnace, covering the gold alloy tube blank with copper foil, burying it in charcoal for annealing, and rapidly cooling it to obtain an annealed tube blank;
[0011] Step 5: boring with a tool having an outer diameter of 10 to 15 mm until the inner surface roughness Ra≤1.6, and turning the outer surface to obtain a bored gold alloy tube blank;
[0012] Step 6: cold-processing the bored gold alloy tube blank with a rotary forging machine to obtain a rotary forged tube;
[0013] Step 7, subjecting the rotary forged pipe to intermediate annealing treatment, and then subjecting the pipe to multiple cold rolling processes to obtain a cold rolled pipe;
[0014] Step 8, subjecting the cold-rolled tube to a heating annealing treatment, and performing a multi-pass cold drawing process using a moving mandrel to obtain a cold-drawn tube;
[0015] Step nine: vacuum annealing the cold-drawn tube to obtain an electrical contact gold alloy thick-walled thin tube.
[0016] The above-mentioned method for preparing a thick-walled thin tube of electrical contact gold alloy is characterized in that, in step 1, the outer diameter of the cylindrical gold alloy ingot is 40-60 mm and the length is 80-100 mm.
[0017] The above-mentioned method for preparing a thick-walled thin tube of an electrical contact gold alloy is characterized in that, in step 2, specifically comprising: firstly casting an ingot after surface treatment on a T 热锻 After heating under temperature conditions, the material is roughened to 40-50 mm in the length direction, then turned 90°, forged and stretched to 80-110 mm in the circumferential direction, and the stretched material is placed at T 热锻 After keeping warm under temperature conditions, the above-mentioned roughening and drawing are repeated to obtain a round rod with a diameter of 25 to 35 mm. The round rod is forged through a forging die with a hole diameter of 22 to 32 mm, finely straightened and cooled to obtain a gold alloy rod blank.
[0018] The above-mentioned method for preparing a thick-walled thin tube of electrical contact gold alloy is characterized in that T 热锻 =700℃, heating time is 1.5h, and holding time is 0.5h.
[0019] The above-mentioned method for preparing thick-walled thin tubes of electrical contact gold alloy is characterized in that, in step three, the turning thickness of the surface oxide layer removed and folded is 1.0 to 1.5 mm; in step three, the centering hole after leveling and the turning to remove the surface oxide layer and folding also include cutting according to a preset length, and the preset length is 120 to 180 mm; in step four, the annealing temperature is 700°C and the annealing time is 1 hour.
[0020] The above-mentioned method for preparing thick-walled thin tubes of electrical contact gold alloy is characterized in that, in step five, the turning thickness is 0.5 mm; in step five, the size of the gold alloy tube blank after boring is: outer diameter 18-28 mm, inner diameter 10-15 mm, length 120-180 mm.
[0021] The above-mentioned method for preparing thick-walled thin tubes of electrical contact gold alloy is characterized in that step six specifically includes: using spring steel as a core rod, transformer oil as a lubricating oil, and a copper tube as a push rod, and performing rotary forging according to the outer diameter being reduced by 2 mm per pass and the wall thickness being reduced by 0.5 to 0.6 mm per pass to obtain a rotary forged tube with an outer diameter of 12 to 14 mm and an inner diameter of 7 to 8 mm.
[0022] The above-mentioned method for preparing thick-walled thin tubes of electrical contact gold alloy is characterized in that, in step seven, the intermediate annealing treatment temperature is 650°C and the time is 1 hour; in step seven, during the cold rolling process, the outer diameter is reduced by 1.3 to 2.0 mm per pass, and the wall thickness is reduced by 0.2 to 0.5 mm per pass; in step seven, the size of the tube after cold rolling is: outer diameter 5.0 to 5.5 mm, inner diameter 3.0 to 4.0 mm.
[0023] The above-mentioned method for preparing thick-walled thin tubes of electrical contact gold alloy is characterized in that, in step eight, the heating annealing treatment temperature is 650°C and the time is 1 hour; in step eight, during the cold drawing process, the outer diameter is reduced by 1.0 to 1.5 mm per pass, and the wall thickness is reduced by 0.1 to 0.15 mm per pass; in step eight, the size of the tube after cold drawing is: outer diameter 2.5 to 4.0 mm, inner diameter 1.2 to 2.0 mm.
[0024] The above-mentioned method for preparing thick-walled thin tubes of electrical contact gold alloy is characterized in that, in step nine, the vacuum annealing temperature is 320° C. and the heating time is 1 hour.
[0025] Compared with the prior art, the present invention has the following advantages:
[0026] 1. The method for preparing the thick-walled fine tube of the electrical contact gold alloy of the present invention comprises hot forging a cylindrical gold alloy ingot, cold working the bored gold alloy tube blank by a rotary forging machine, and cold drawing the cold rolled tube by a floating core head. The method can effectively avoid the defects of uneven microstructure and mechanical cracking of the gold alloy thick-walled fine tube prepared by the existing method, and has the characteristics of uniform microstructure and high inner surface finish and high production efficiency.
[0027] 2. The method for preparing the electrical contact gold alloy thick-walled fine tube of the present invention comprises performing hot forging including two roughening and drawing processes on the ingot after polishing, which can effectively eliminate microscopic pores and increase density, and the obtained gold alloy thick-walled fine tube has more uniform organizational properties.
[0028] 3. The method for preparing the thick-walled thin tube of the electrical contact gold alloy of the present invention comprises using a rotary forging machine to perform multiple cold working steps, which can effectively control the compressive stress deformation of the tube blank and improve the hardness of the product alloy.
[0029] 4. The method for preparing the thick-walled thin tube of the electrical contact gold alloy of the present invention comprises cold drawing the cold-rolled tube through a movable core head, which can make the inner and outer surfaces of the tube deform evenly, effectively eliminate defects such as wrinkles on the inner surface, improve the smoothness of the inner surface, and avoid cracking caused by subsequent turning.
[0030] 5. The method for preparing the thick-walled thin tube of the electrical contact gold alloy of the present invention includes vacuum annealing the tube after cold drawing, which can promote the uniformity of the circumferential stress of the tube and has the characteristics of higher precision and better uniformity.
[0031] 6. The method for preparing the electrical contact gold alloy thick-walled thin tube of the present invention is simple to operate, has high production efficiency, and is conducive to popularization and application.
[0032] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a schematic diagram of the cold working process using a rotary forging machine in step six of the present invention.
[0034] Figure 2 for Figure 1 Side view of.
[0035] Figure 3 It is a schematic diagram of the partial structure of the rotary forging die.
[0036] Figure 4 for Figure 3 Side view of.
[0037] Figure 5 This is a schematic diagram of the processing process of cold drawing by a movable core head in step eight of the present invention.
[0038] Figure 6 Schematic diagram of the drawing outer mold structure.
[0039] Figure 7 Schematic diagram of the drawing inner mold structure.
[0040] Figure 8 It is a cross-sectional view of a gold alloy thick-walled thin tube prepared by a common method in the background technology.
[0041] Fig. 9 This is a cross-sectional view of the electrical contact gold alloy thick-walled thin tube of Example 1.
[0042] Description of Reference Numerals
[0043] 1—mandrel; 2—copper tube mandrel; 3—tube blank;
[0044] 4—rotary forging die; 41—diameter-changing belt part; 42—sizing belt part;
[0045] 5—drawing inner die; 6—drawing outer die; 51—drawing inner die reducing part;
[0046] 52—drawing inner die sizing part; 53—drawing inner die stabilizing part; 61—drawing outer die reducing part;
[0047] 62—Pull the outer mold to fix the neck. DETAILED DESCRIPTION
[0048] Example 1
[0049] This embodiment provides a method for preparing a thick-walled thin tube of an electrical contact gold alloy, which specifically includes:
[0050] Step 1, lathe the surface of a cylindrical gold alloy ingot; the cylindrical gold alloy ingot has an outer diameter of 50 mm and a length of 100 mm; the cylindrical gold alloy ingot is a vacuum induction melting ingot; in this embodiment, the cylindrical gold alloy ingot can also be an arc melting ingot;
[0051] Step 2: hot forging the polished ingot to eliminate micro defects such as internal shrinkage cavities and segregation, including:
[0052] Step 201, placing the polished ingot in a resistance furnace at 700° C. and heating for 1.5 hours;
[0053] Step 202, the heated ingot is roughened to 50 mm in the length direction by a fast forging machine, then turned 90 degrees, and forged and stretched to 100 mm in the circumferential direction;
[0054] Step 203, returning the drawn material to a 700° C. resistance furnace for 0.5 h;
[0055] Step 204, according to step 202, the material after being returned to the furnace for heat preservation is forged, upset and stretched again to obtain a round bar with a diameter of 30 mm;
[0056] Step 205, using a forging die with a hole diameter of 28 mm, finishing and straightening the round rod into a rod blank, and putting it into water for rapid cooling to obtain a gold alloy rod blank;
[0057] Step 3: Use a lathe to cut the shrinkage holes at both ends of the gold alloy rod blank, level it and then center it, cut it according to the preset length of 140 mm, clamp both ends, remove the surface oxide layer and folding by turning, and then drill a hole with an outer diameter of 12 mm to obtain a gold alloy tube blank; the turning thickness is 1.5 mm;
[0058] Step 4: Place a charcoal box in the resistance furnace, and as the furnace heats up, wrap the gold alloy tube blank with copper foil, bury it in the charcoal in the resistance furnace at 700°C, perform heat preservation annealing for 1 hour, take it out of the furnace and put it into water for rapid cooling to obtain the annealed tube blank;
[0059] Step 5: boring with a tool with an outer diameter of 13 mm until the inner surface roughness Ra≤1.6, centering the hole, turning the outer surface by 0.5 mm, and obtaining a bored gold alloy tube blank; the bored gold alloy tube blank has the following dimensions: outer diameter 24 mm, inner diameter 13 mm, and length 140 mm;
[0060] Step 6, cold working the bored gold alloy tube blank with a rotary forging machine, specifically comprising: using 5 spring steels with gradually reduced diameters and a length of 500 mm as a mandrel group, using transformer oil as lubricating oil, and using a copper tube as a push rod, inserting the corresponding mandrel into the bored gold alloy tube blank, pushing the alloy tube blank and the mandrel through the rotary forging die by the push rod, and rotary forging is performed according to the outer diameter being reduced by 2 mm per pass and the wall thickness being reduced by 0.5 mm per pass. During the rotary forging process, the tube is cut off when the length is greater than 300 mm to obtain a rotary forged tube with an outer diameter of 14 mm and an inner diameter of 8 mm; the mandrel is replaced between two adjacent rotary forging passes;
[0061] The inner diameter of the rotary forging die and the outer diameter of the mandrel for each pass are as follows:
[0062] 1st pass: rotary forging die 22mm, mandrel 12mm;
[0063] Second pass: rotary forging die 20mm, mandrel 11mm;
[0064] The third pass: rotary forging die 18mm, mandrel 10mm;
[0065] 4th pass: rotary forging die 16mm, mandrel 9mm;
[0066] Pass 5: swaging die 14mm, mandrel 8mm;
[0067] In step 6, the cold working process using a rotary forging machine is as follows Figure 1 and Figure 2 As shown, the mandrel 1 is inserted into the tube blank 3, and the copper tube push rod 2 pushes the tube blank 3 and the mandrel 1 forward, so that the tube blank 3 flows toward the die feed end of the rotary forging die 4;
[0068] The partial structure of the rotary forging die 4 is as follows Figure 3 As shown, Figure 4 for Figure 3 The rotary forging die 4 includes a variable diameter belt portion 41 and a fixed diameter belt portion 42 connected to each other, the large-diameter portion of the variable diameter belt portion 41 is away from the fixed diameter belt portion 42, and the small-diameter portion of the variable diameter belt portion 41 is connected to the fixed diameter belt portion 42;
[0069] The radius of the variable diameter band portion 41 is in the range of 50 to 60 mm, and the length of the fixed diameter band portion 42 is in the range of 8 to 10 mm.
[0070] Step 7, subjecting the rotary forged pipe to a heating annealing treatment at a temperature of 650° C. for 1 hour to eliminate processing stress, and then subjecting the pipe to a cold rolling process for multiple passes to obtain a cold rolled pipe; in the multiple cold rolling processes, the outer diameter is reduced by 1.5 to 2.0 mm per pass, and the wall thickness is reduced by 0.3 to 0.5 mm per pass; the dimensions of the cold rolled pipe are: an outer diameter of 5.5 mm and an inner diameter of 3.8 mm;
[0071] Pass 1: outer diameter 12mm, mandrel 7mm;
[0072] Second pass: outer diameter 10mm, mandrel 6mm;
[0073] Pass 3: outer diameter 8mm, mandrel 5mm;
[0074] 4th pass: outer diameter 6.5mm, mandrel 4.3mm;
[0075] Pass 5: outer diameter 5.5mm, mandrel 3.8mm;
[0076] Step 8, subjecting the cold-rolled tube to a heating annealing treatment at a temperature of 650° C. for 1 hour, and subjecting the tube to a cold-drawn tube by a moving mandrel; during the cold-drawing process, the outer diameter is reduced by 1.0 to 1.5 mm per pass, and the wall thickness is reduced by 0.1 mm per pass; the dimensions of the cold-drawn tube are: outer diameter 3.0 mm, inner diameter 1.7 mm;
[0077] 1st pass: outer diameter 4mm, inner diameter 2.5mm;
[0078] Second pass: outer diameter 3mm, inner diameter 1.7mm;
[0079] The schematic diagram of the cold drawing process by the floating core head in step eight is as follows Figure 5As shown, the inner drawing die 5 is placed in the pipe, and force is applied to cause the pipe to pass through the outer drawing die 6. Under the action of the friction force inside the pipe and the reaction force during deformation, the inner drawing die 5 and the pipe reach a dynamic balance, and the inner diameter of the pipe is controlled by the inner drawing die 5, and the outer diameter of the pipe is controlled by the outer drawing die 6.
[0080] The drawing outer die 6 comprises a drawing outer die reducing portion 61 and a drawing outer die fixed neck portion 62, and the length of the drawing outer die fixed neck portion 62 is 3 to 4 mm;
[0081] The inner drawing die 5 comprises an inner drawing die reducing portion 51, an inner drawing die sizing portion 52 and an inner drawing die stabilizing portion 53, wherein the small diameter portion of the inner drawing die reducing portion 51 is connected to the inner drawing die sizing portion 52, and the large diameter portion of the inner drawing die reducing portion 51 is connected to the inner drawing die stabilizing portion 53;
[0082] The length of the inner drawing die sizing portion 52 is 4 to 4.5 mm, the length of the inner drawing die reducing portion 51 is 2 to 3.5 mm, and the length of the inner drawing die stabilizing portion 53 is 5 to 5.5 mm;
[0083] The number of the drawing inner dies is consistent with the number of passes. In each pass, the diameter of the drawing inner die sizing portion 52 is equal to the inner diameter of the tube after each drawing pass, and the diameter of the drawing inner die stabilizing portion 53 is 0.2 mm smaller than the inner diameter of the tube before each drawing pass. The structural schematic diagram of the drawing outer die 6 and the drawing inner die 5 is as shown in FIG. Figure 6 and Figure 7 shown.
[0084] Step nine: placing the cold-drawn tube in a vacuum annealing furnace at 320° C. and heating it for 1 hour to perform stress homogenization annealing treatment to obtain an electrical contact gold alloy thick-walled thin tube.
[0085] The electrical contact gold alloy thick-walled thin tube of this embodiment meets the technical standard YS / T 207-2013 "Precious metal and alloy tubes for conductive rings".
[0086] Figure 8 is a cross-sectional view of a gold alloy thick-walled thin tube prepared by a common method in the background technology, Fig. 9 is a cross-sectional view of the electrical contact gold alloy thick-walled thin tube of this embodiment, compared with Figure 8 and Fig. 9 It can be seen that the electrical contact gold alloy thick-walled thin tube of this embodiment has no wrinkles and cracks, indicating that the method of the present invention can effectively avoid the wrinkles and cracks caused by the traditional method and has the characteristic of higher yield.
[0087] Example 2
[0088] This embodiment provides a method for preparing a thick-walled thin tube of an electrical contact gold alloy, which specifically includes:
[0089] Step 1, lathe the surface of a cylindrical gold alloy ingot; the cylindrical gold alloy ingot has an outer diameter of 40 mm and a length of 80 mm; the cylindrical gold alloy ingot is a vacuum induction melting ingot;
[0090] Step 2: hot forging the polished ingot, specifically including:
[0091] Step 201, placing the polished ingot in a resistance furnace at 700° C. and heating for 1.5 hours;
[0092] Step 202, the heated ingot is roughened to 40 mm in the length direction by a fast forging machine, then turned 90 degrees, and forged and stretched to 80 mm in the circumferential direction;
[0093] Step 203, returning the drawn material to a 700° C. resistance furnace for 0.5 h;
[0094] Step 204, according to step 202, the material after being returned to the furnace for heat preservation is forged, upset and stretched again to obtain a round bar with a diameter of 25 mm;
[0095] Step 205, using a forging die with a hole diameter of 22 mm, finishing and straightening the round rod into a rod blank, and putting it into water for rapid cooling to obtain a gold alloy rod blank;
[0096] Step 3: Use a lathe to cut the shrinkage holes at both ends of the gold alloy rod blank, level it and then center it, cut it according to the preset length of 128 mm, clamp both ends, remove the surface oxide layer and folding by turning, and then drill a hole with a drill bit with an outer diameter of 9 mm to obtain a gold alloy tube blank; the turning thickness is 1.5 mm;
[0097] Step 4: Place a charcoal box in the resistance furnace, and as the furnace heats up, wrap the gold alloy tube blank with copper foil, bury it in the charcoal in the resistance furnace at 700°C, perform heat preservation annealing for 1 hour, take it out of the furnace and put it into water for rapid cooling to obtain the annealed tube blank;
[0098] Step 5: boring with a tool with an outer diameter of 10 mm until the inner surface roughness Ra≤1.6, centering the hole, turning the outer surface by 0.5 mm, and obtaining a bored gold alloy tube blank; the bored gold alloy tube blank has the following dimensions: outer diameter 18 mm, inner diameter 10 mm, and length 128 mm;
[0099] Step 6: Use a rotary forging machine to cold-process the bored gold alloy tube blank, specifically including: using 4 spring steels with gradually reduced diameters and a length of 500 mm as a mandrel group, using transformer oil as lubricating oil, and using a copper tube as a push rod, inserting the corresponding mandrel into the bored gold alloy tube blank, pushing the alloy tube blank and the mandrel through the rotary forging die by the push rod, and rotary forging is performed according to the outer diameter being reduced by 2 mm per pass and the wall thickness being reduced by 0.5 mm per pass. When the length of the tube is greater than 300 mm during the rotary forging process, it is cut off to obtain a rotary forging tube with an outer diameter of 12 mm and an inner diameter of 7 mm; the mandrel is replaced between two adjacent rotary forging passes; the inner diameter of the rotary forging die and the outer diameter of the mandrel are as follows:
[0100] 1st pass: rotary forging die 18mm, mandrel 10mm;
[0101] Second pass: rotary forging die 16mm, mandrel 9mm;
[0102] Pass 3: swaging die 14mm, mandrel 8mm;
[0103] The 4th pass: rotary forging die 12mm, mandrel 7mm;
[0104] Step 7, subjecting the rotary forged pipe to a heating annealing treatment at a temperature of 650° C. for 1 hour, and then subjecting the pipe to a multi-pass cold rolling process to obtain a cold-rolled pipe; in the multi-pass cold rolling process, the outer diameter is reduced by 1.5 to 2.0 mm per pass, and the wall thickness is reduced by 0.3 to 0.5 mm per pass; the dimensions of the cold-rolled pipe are: an outer diameter of 5.0 mm and an inner diameter of 3.2 mm;
[0105] 1st pass: outer diameter 10mm, mandrel 6mm;
[0106] Pass 2: outer diameter 8mm, mandrel 5mm;
[0107] The third pass: outer diameter 6.5mm, mandrel 4.1mm;
[0108] 4th pass: outer diameter 5mm, mandrel 3.2mm;
[0109] Step 8, subjecting the cold-rolled tube to a heating annealing treatment at a temperature of 650° C. for 1 hour, and subjecting the tube to a cold-drawn tube by a moving mandrel; during the cold-drawing process, the outer diameter is reduced by 1.0 to 1.2 mm per pass, and the wall thickness is reduced by 0.1 mm per pass; the dimensions of the cold-drawn tube are: outer diameter 2.8 mm, inner diameter 1.4 mm;
[0110] Pass 1: outer diameter 3.8mm, inner diameter 2.2mm;
[0111] Pass 2: outer diameter 2.8mm, inner diameter 1.4mm;
[0112] Step nine: placing the cold-drawn tube in a vacuum annealing furnace at 320° C. and heating it for 1 hour to perform stress homogenization annealing treatment to obtain an electrical contact gold alloy thick-walled thin tube.
[0113] The electrical contact gold alloy thick-walled thin tube of this embodiment meets the technical standard YS / T 207-2013 "Precious metal and alloy tubes for conductive rings".
[0114] Example 3
[0115] This embodiment provides a method for preparing a thick-walled thin tube of an electrical contact gold alloy, which specifically includes:
[0116] Step 1, lathe the surface of a cylindrical gold alloy ingot; the cylindrical gold alloy ingot has an outer diameter of 60 mm and a length of 100 mm; the cylindrical gold alloy ingot is a vacuum induction melting ingot;
[0117] Step 2: hot forging the polished ingot, specifically including:
[0118] Step 201, placing the polished ingot in a resistance furnace at 700° C. and heating for 1.5 hours;
[0119] Step 202, the heated ingot is roughened to 50 mm in the length direction by a fast forging machine, then turned 90 degrees, and forged and stretched to 110 mm in the circumferential direction;
[0120] Step 203, returning the drawn material to a 700° C. resistance furnace for 0.5 h;
[0121] Step 204, according to step 202, the material after being returned to the furnace for heat preservation is forged, upset and stretched again to obtain a round bar with a diameter of 35 mm;
[0122] Step 205, using a forging die with a hole diameter of 32 mm, finishing and straightening the round rod into a rod blank, and putting it into water for rapid cooling to obtain a gold alloy rod blank;
[0123] Step 3: Use a lathe to cut the shrinkage holes at both ends of the gold alloy rod blank, level it and then center it, cut it according to the preset length of 140 mm, clamp both ends, remove the surface oxide layer and folding by turning, and then drill a hole with an outer diameter of 14 mm to obtain a gold alloy tube blank; the turning thickness is 1.5 mm;
[0124] Step 4: Place a charcoal box in the resistance furnace, and as the furnace heats up, wrap the gold alloy tube blank with copper foil, bury it in the charcoal in the resistance furnace at 700°C, perform heat preservation annealing for 1 hour, take it out of the furnace and put it into water for rapid cooling to obtain the annealed tube blank;
[0125] Step 5: boring with a tool with an outer diameter of 15 mm until the inner surface roughness Ra≤1.6, centering the hole, turning the outer surface by 0.5 mm, and obtaining a bored gold alloy tube blank; the bored gold alloy tube blank has the following dimensions: outer diameter 28 mm, inner diameter 15 mm, and length 150 mm;
[0126] Step 6: cold-process the bored gold alloy tube blank with a rotary forging machine, specifically including: using 7 spring steels with gradually reduced diameters and a length of 600 mm as a mandrel group, using transformer oil as lubricating oil, and using a copper tube as a push rod, inserting the corresponding mandrel into the bored gold alloy tube blank, pushing the alloy tube blank and the mandrel through the rotary forging die by the push rod, and rotary forging is performed according to the outer diameter being reduced by 2 mm per pass and the wall thickness being reduced by 0.5 to 0.6 mm per pass. During the rotary forging process, the tube is cut off when the length is greater than 300 mm to obtain a rotary forged tube with an outer diameter of 14 mm and an inner diameter of 8 mm; the mandrel is replaced between two adjacent rotary forging passes; the inner diameter of the rotary forging die and the outer diameter of the mandrel are as follows:
[0127] 1st pass: rotary forging die 26mm, mandrel 13.8mm;
[0128] Second pass: rotary forging die 24mm, mandrel 13mm;
[0129] The third pass: rotary forging die 22mm, mandrel 12mm;
[0130] The 4th pass: rotary forging die 20mm, mandrel 11mm;
[0131] The fifth pass: rotary forging die 18mm, mandrel 10mm;
[0132] The 6th pass: rotary forging die 16mm, mandrel 9mm;
[0133] Pass 7: swaging die 14mm, mandrel 8mm;
[0134] Step 7, subjecting the rotary forged pipe to a heating annealing treatment at a temperature of 650° C. for 1 hour, and then subjecting the pipe to a multi-pass cold rolling process to obtain a cold-rolled pipe; in the multi-pass cold rolling process, the outer diameter is reduced by 1.5 to 2.0 mm per pass, and the wall thickness is reduced by 0.2 to 0.5 mm per pass; the dimensions of the cold-rolled pipe are: an outer diameter of 5.5 mm and an inner diameter of 3.5 mm;
[0135] Pass 1: outer diameter 12mm, mandrel 7mm;
[0136] Second pass: outer diameter 10mm, mandrel 6mm;
[0137] Pass 3: outer diameter 8mm, mandrel 5mm;
[0138] 4th pass: outer diameter 6.5mm, mandrel 4.1mm;
[0139] Pass 5: outer diameter 5.5mm, mandrel 3.5mm;
[0140] Step 8, subjecting the cold-rolled tube to a heating annealing treatment at a temperature of 650° C. for 1 hour, and subjecting the tube to a cold-drawn tube by a moving mandrel; during the cold-drawing process, the outer diameter is reduced by 1.0 to 1.2 mm per pass, and the wall thickness is reduced by 0.1 mm per pass; the dimensions of the cold-drawn tube are: outer diameter 3.5 mm, inner diameter 1.5 mm;
[0141] Pass 1: outer diameter 4.3mm, inner diameter 2.2mm;
[0142] Second pass: outer diameter 3.5mm, inner diameter 1.5mm;
[0143] Step nine: placing the cold-drawn tube in a vacuum annealing furnace at 320° C. and heating it for 1 hour to perform stress homogenization annealing treatment to obtain an electrical contact gold alloy thick-walled thin tube.
[0144] The electrical contact gold alloy thick-walled thin tube of this embodiment meets the technical standard YS / T 207-2013 "Precious metal and alloy tubes for conductive rings".
[0145] Example 4
[0146] This embodiment provides a method for preparing a thick-walled thin tube of an electrical contact gold alloy, which specifically includes:
[0147] Step 1, lathe the surface of a cylindrical gold alloy ingot; the cylindrical gold alloy ingot has an outer diameter of 40 mm and a length of 100 mm; the cylindrical gold alloy ingot is a vacuum induction melting ingot;
[0148] Step 2: hot forging the polished ingot, specifically including:
[0149] Step 201, placing the polished ingot in a resistance furnace at 700° C. and heating for 1.5 hours;
[0150] Step 202, the heated ingot is roughened to 40 mm in the length direction by a fast forging machine, then turned 90 degrees, and forged and stretched to 100 mm in the circumferential direction;
[0151] Step 203, returning the drawn material to a 700° C. resistance furnace for 0.5 h;
[0152] Step 204, according to step 202, the material after being returned to the furnace for heat preservation is forged, upset and stretched again to obtain a round bar with a diameter of 30 mm;
[0153] Step 205, using a forging die with a hole diameter of 26 mm, finishing and straightening the round rod into a rod blank, and putting it into water for rapid cooling to obtain a gold alloy rod blank;
[0154] Step 3: Use a lathe to cut the shrinkage holes at both ends of the gold alloy rod blank, level it and then center it, cut it according to the preset length of 160 mm, clamp both ends, remove the surface oxide layer and folding by turning, and then drill a hole with an outer diameter of 11 mm to obtain a gold alloy tube blank; the turning thickness is 1.5 mm;
[0155] Step 4: Place a charcoal box in the resistance furnace, and as the furnace heats up, wrap the gold alloy tube blank with copper foil, bury it in the charcoal in the resistance furnace at 700°C, perform heat preservation annealing for 1 hour, take it out of the furnace and put it into water for rapid cooling to obtain the annealed tube blank;
[0156] Step 5: boring with a tool with an outer diameter of 12 mm until the inner surface roughness Ra≤1.6, centering the hole, turning the outer surface by 0.5 mm, and obtaining a bored gold alloy tube blank; the bored gold alloy tube blank has the following dimensions: outer diameter 22 mm, inner diameter 12 mm, and length 160 mm;
[0157] Step 6: Use a rotary forging machine to cold-process the bored gold alloy tube blank, specifically including: using 4 spring steels with gradually reduced diameters and a length of 600 mm as a mandrel group, using transformer oil as lubricating oil, and using a copper tube as a push rod, inserting the corresponding mandrel into the bored gold alloy tube blank, pushing the alloy tube blank and the mandrel through the rotary forging die by the push rod, and rotary forging is performed according to the outer diameter being reduced by 2 mm per pass and the wall thickness being reduced by 0.5 mm per pass. During the rotary forging process, the tube is cut off when the length is greater than 300 mm to obtain a rotary forged tube with an outer diameter of 14 mm and an inner diameter of 8 mm; the mandrel is replaced between two adjacent rotary forging passes; the inner diameter of the rotary forging die and the outer diameter of the mandrel are as follows:
[0158] 1st pass: rotary forging die 20mm, mandrel 11mm;
[0159] Second pass: rotary forging die 18mm, mandrel 10mm;
[0160] The third pass: rotary forging die 16mm, mandrel 9mm;
[0161] Pass 4: swaging die 14mm, mandrel 8mm;
[0162] Step 7, subjecting the rotary forged pipe to a heating annealing treatment at a temperature of 650° C. for 1 hour, and then subjecting the pipe to a multi-pass cold rolling process to obtain a cold-rolled pipe; in the multi-pass cold rolling process, the outer diameter is reduced by 1.5 to 2.0 mm per pass, and the wall thickness is reduced by 0.3 to 0.5 mm per pass; the dimensions of the cold-rolled pipe are: an outer diameter of 5.0 mm and an inner diameter of 3.2 mm;
[0163] 1st pass: outer diameter 10mm, mandrel 6mm;
[0164] Pass 2: outer diameter 8mm, mandrel 5mm;
[0165] The third pass: outer diameter 6.5mm, mandrel 4.1mm;
[0166] 4th pass: outer diameter 5mm, mandrel 3.2mm;
[0167] Step 8, subjecting the cold-rolled tube to a heating annealing treatment at a temperature of 650° C. for 1 hour, and subjecting the tube to a cold-drawn tube by a moving mandrel; during the cold-drawing process, the outer diameter is reduced by 1.0 to 1.5 mm per pass, and the wall thickness is reduced by 0.1 to 0.15 mm per pass; the dimensions of the cold-drawn tube are: an outer diameter of 2.5 mm and an inner diameter of 1.2 mm;
[0168] Pass 1: outer diameter 3.5mm, inner diameter 2.0mm;
[0169] Pass 2: outer diameter 2.5mm, inner diameter 1.2mm;
[0170] Step nine: placing the cold-drawn tube in a vacuum annealing furnace at 320° C. and heating it for 1 hour to perform stress homogenization annealing treatment to obtain an electrical contact gold alloy thick-walled thin tube.
[0171] The electrical contact gold alloy thick-walled thin tube of this embodiment meets the technical standard YS / T 207-2013 "Precious metal and alloy tubes for conductive rings".
[0172] Example 5
[0173] This embodiment provides a method for preparing a thick-walled thin tube of an electrical contact gold alloy, which specifically includes:
[0174] Step 1, lathe the surface of a cylindrical gold alloy ingot; the cylindrical gold alloy ingot has an outer diameter of 50 mm and a length of 90 mm; the cylindrical gold alloy ingot is a vacuum induction melting ingot;
[0175] Step 2: hot forging the polished ingot, specifically including:
[0176] Step 201, placing the polished ingot in a resistance furnace at 700° C. and heating for 1.5 hours;
[0177] Step 202, roughening the heated ingot to 40 mm in the length direction by a fast forging machine, then turning it 90 degrees, and forging and stretching it to 90 mm in the circumferential direction;
[0178] Step 203, returning the drawn material to a 700° C. resistance furnace for 0.5 h;
[0179] Step 204, according to step 202, the material after being returned to the furnace for heat preservation is forged, upset and stretched again to obtain a round bar with a diameter of 28 mm;
[0180] Step 205, using a forging die with a hole diameter of 25 mm, finishing and straightening the round rod into a rod blank, and putting it into water for rapid cooling to obtain a gold alloy rod blank;
[0181] Step 3: Use a lathe to cut the shrinkage holes at both ends of the gold alloy rod blank, level it and then center it, cut it according to the preset length of 138 mm, clamp both ends, remove the surface oxide layer and folding by turning, and then drill a hole with an outer diameter of 11 mm to obtain a gold alloy tube blank; the turning thickness is 1.0 mm;
[0182] Step 4: Place a charcoal box in the resistance furnace, and as the furnace heats up, wrap the gold alloy tube blank with copper foil, bury it in the charcoal in the resistance furnace at 700°C, perform heat preservation annealing for 1 hour, take it out of the furnace and put it into water for rapid cooling to obtain the annealed tube blank;
[0183] Step 5: boring with a tool with an outer diameter of 12 mm until the inner surface roughness Ra≤1.6, centering the hole, turning the outer surface by 0.5 mm, and obtaining a bored gold alloy tube blank; the bored gold alloy tube blank has the following dimensions: outer diameter 22 mm, inner diameter 12 mm, and length 160 mm;
[0184] Step 6: cold-process the bored gold alloy tube blank with a rotary forging machine, specifically including: using 7 spring steels with gradually reduced diameters and a length of 500 mm as a mandrel group, using transformer oil as lubricating oil, and using a copper tube as a push rod, inserting the corresponding mandrel into the bored gold alloy tube blank, pushing the alloy tube blank and the mandrel through the rotary forging die by the push rod, and rotary forging is performed according to the outer diameter being reduced by 2 mm per pass and the wall thickness being reduced by 0.5 mm per pass. When the length of the tube is greater than 300 mm during the rotary forging process, it is cut off to obtain a rotary forging tube with an outer diameter of 14 mm and an inner diameter of 8 mm; the mandrel is replaced between two adjacent rotary forging passes; the inner diameter of the rotary forging die and the outer diameter of the mandrel are as follows:
[0185] 1st pass: rotary forging die 20mm, mandrel 11mm;
[0186] Second pass: rotary forging die 18mm, mandrel 10mm;
[0187] The third pass: rotary forging die 16mm, mandrel 9mm;
[0188] Pass 4: swaging die 14mm, mandrel 8mm;
[0189] Step 7, subjecting the rotary forged pipe to a heating annealing treatment at a temperature of 650° C. for 1 hour, and then subjecting the pipe to a multi-pass cold rolling process to obtain a cold-rolled pipe; in the multi-pass cold rolling process, the outer diameter is reduced by 1.3 to 2.0 mm per pass, and the wall thickness is reduced by 0.2 to 0.5 mm per pass; the dimensions of the cold-rolled pipe are: an outer diameter of 5.2 mm and an inner diameter of 3.2 mm;
[0190] 1st pass: outer diameter 10mm, mandrel 6mm;
[0191] Pass 2: outer diameter 8mm, mandrel 5mm;
[0192] The third pass: outer diameter 6.5mm, mandrel 4.1mm;
[0193] Pass 4: outer diameter 5.2mm, mandrel 3.2mm;
[0194] Step 8, subjecting the cold-rolled tube to a heating annealing treatment at a temperature of 650° C. for 1 hour, and subjecting the tube to a cold-drawn tube by a moving mandrel; during the cold-drawing process, the outer diameter is reduced by 1.0 to 1.5 mm per pass, and the wall thickness is reduced by 0.1 to 0.15 mm per pass; the dimensions of the cold-drawn tube are: outer diameter 3.2 mm, inner diameter 1.6 mm;
[0195] Pass 1: outer diameter 4.0mm, inner diameter 2.2mm;
[0196] Pass 2: outer diameter 3.2mm, inner diameter 1.6mm;
[0197] Step nine: placing the cold-drawn tube in a vacuum annealing furnace at 320° C. and heating it for 1 hour to perform stress homogenization annealing treatment to obtain an electrical contact gold alloy thick-walled thin tube.
[0198] The electrical contact gold alloy thick-walled thin tube of this embodiment meets the technical standard YS / T 207-2013 "Precious metal and alloy tubes for conductive rings".
[0199] Example 6
[0200] This embodiment provides a method for preparing a thick-walled thin tube of an electrical contact gold alloy, which specifically includes:
[0201] Step 1, lathe the surface of a cylindrical gold alloy ingot; the cylindrical gold alloy ingot has an outer diameter of 60 mm and a length of 80 mm; the cylindrical gold alloy ingot is a vacuum induction melting ingot;
[0202] Step 2: hot forging the polished ingot, specifically including:
[0203] Step 201, placing the polished ingot in a resistance furnace at 700° C. and heating for 1.5 hours;
[0204] Step 202, the heated ingot is roughened to 40 mm in the length direction by a fast forging machine, then turned 90 degrees, and forged and stretched to 110 mm in the circumferential direction;
[0205] Step 203, returning the drawn material to a 700° C. resistance furnace for 0.5 h;
[0206] Step 204, according to step 202, the material after being returned to the furnace for heat preservation is forged, upset and stretched again to obtain a round bar with a diameter of 28 mm;
[0207] Step 205, using a forging die with a hole diameter of 25 mm, finishing and straightening the round rod into a rod blank, and putting it into water for rapid cooling to obtain a gold alloy rod blank;
[0208] Step 3: Use a lathe to cut the shrinkage holes at both ends of the gold alloy rod blank, level it and then center it, cut it according to the preset length of 178 mm, clamp both ends, remove the surface oxide layer and folding by turning, and then drill a hole with a drill bit with an outer diameter of 10 mm to obtain a gold alloy tube blank; the turning thickness is 1.5 mm;
[0209] Step 4: Place a charcoal box in the resistance furnace, and as the furnace heats up, wrap the gold alloy tube blank with copper foil, bury it in the charcoal in the resistance furnace at 700°C, perform heat preservation annealing for 1 hour, take it out of the furnace and put it into water for rapid cooling to obtain the annealed tube blank;
[0210] Step 5: boring with a tool having an outer diameter of 11 mm until the inner surface roughness Ra≤1.6, centering the hole, turning the outer surface by 0.5 mm, and obtaining a bored gold alloy tube blank; the bored gold alloy tube blank has the following dimensions: outer diameter 22 mm, inner diameter 11 mm, and length 178 mm;
[0211] Step 6: cold-process the bored gold alloy tube blank with a rotary forging machine, specifically including: using 7 spring steels with gradually reduced diameters and a length of 600 mm as a mandrel group, using transformer oil as lubricating oil, and using a copper tube as a push rod, inserting the corresponding mandrel into the bored gold alloy tube blank, pushing the alloy tube blank and the mandrel through the rotary forging die through the push rod, and rotary forging is performed according to the outer diameter being reduced by 2 mm per pass and the wall thickness being reduced by 0.5 mm per pass. When the length of the tube is greater than 300 mm during the rotary forging process, it is cut off to obtain a rotary forging tube with an outer diameter of 14 mm and an inner diameter of 7 mm; the mandrel is replaced between two adjacent rotary forging passes; the inner diameter of the rotary forging die and the outer diameter of the mandrel are as follows:
[0212] 1st pass: rotary forging die 20mm, mandrel 10mm;
[0213] Second pass: rotary forging die 18mm, mandrel 9mm;
[0214] The third pass: rotary forging die 16mm, mandrel 8mm;
[0215] 4th pass: rotary forging die 14mm, mandrel 7mm;
[0216] Step 7, subjecting the rotary forged pipe to a heating annealing treatment at a temperature of 650° C. for 1 hour, and then subjecting the pipe to a multi-pass cold rolling process to obtain a cold-rolled pipe; in the multi-pass cold rolling process, the outer diameter is reduced by 1.5 to 2.0 mm per pass, and the wall thickness is reduced by 0.35 to 0.5 mm per pass; the dimensions of the cold-rolled pipe are: an outer diameter of 5.5 mm and an inner diameter of 3.0 mm;
[0217] Pass 1: outer diameter 12mm, mandrel 6mm;
[0218] Second pass: outer diameter 10mm, mandrel 5mm;
[0219] The third pass: outer diameter 8.5mm, mandrel 4.5mm;
[0220] Pass 4: outer diameter 7mm, mandrel 3.8mm;
[0221] Pass 5: outer diameter 5.5mm, mandrel 3.0mm;
[0222] Step 8, subjecting the cold-rolled tube to a heating annealing treatment at a temperature of 650° C. for 1 hour, and subjecting the tube to a cold-drawn tube by a moving mandrel; during the cold-drawing process, the outer diameter is reduced by 1.5 mm per pass, and the wall thickness is reduced by 0.15 mm per pass; the dimensions of the cold-drawn tube are: outer diameter 4.0 mm, inner diameter 1.8 mm;
[0223] Pass 1: outer diameter 4.0mm, inner diameter 1.8mm;
[0224] Step nine: placing the cold-drawn tube in a vacuum annealing furnace at 320° C. and heating it for 1 hour to perform stress homogenization annealing treatment to obtain an electrical contact gold alloy thick-walled thin tube.
[0225] The electrical contact gold alloy thick-walled thin tube of this embodiment meets the technical standard YS / T 207-2013 "Precious metal and alloy tubes for conductive rings".
[0226] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a thick-walled thin tube of electrical contact gold alloy, characterized in that: include: Step 1, surface treating the cylindrical gold alloy ingot; Step 2, hot forging the surface treated ingot to obtain a gold alloy bar blank; Step 3, removing the shrinkage holes at both ends of the gold alloy rod blank, leveling and centering the hole, removing the surface oxide layer and folding by turning, and then drilling with a drill bit with an outer diameter of 9 to 14 mm to obtain a gold alloy tube blank; Step 4: placing a charcoal box in a resistance furnace, heating the furnace, covering the gold alloy tube blank with copper foil, burying it in charcoal for annealing, and rapidly cooling it to obtain an annealed tube blank; Step 5: boring with a tool having an outer diameter of 10 to 15 mm until the inner surface roughness Ra≤1.6, and turning the outer surface to obtain a bored gold alloy tube blank; Step 6: cold-processing the bored gold alloy tube blank with a rotary forging machine to obtain a rotary forged tube; Step 7, subjecting the rotary forged pipe to intermediate annealing treatment, and then subjecting the pipe to multiple cold rolling processes to obtain a cold rolled pipe; Step 8, subjecting the cold-rolled tube to a heating annealing treatment, and performing a multi-pass cold drawing process using a moving mandrel to obtain a cold-drawn tube; Step nine: vacuum annealing the cold-drawn tube to obtain an electrical contact gold alloy thick-walled thin tube.
2. The method for preparing a thick-walled thin tube of electrical contact gold alloy according to claim 1, characterized in that: In step 1, the outer diameter of the cylindrical gold alloy ingot is 40-60 mm and the length is 80-100 mm.
3. The method for preparing a thick-walled thin tube of electrical contact gold alloy according to claim 1, characterized in that: Step 2 specifically includes: firstly casting the ingot after surface treatment on T 热锻 After heating under temperature conditions, the material is roughened to 40-50 mm in the length direction, then turned 90°, forged and stretched to 80-110 mm in the circumferential direction, and the stretched material is placed at T 热锻 After keeping warm under temperature conditions, the above-mentioned roughening and drawing are repeated to obtain a round rod with a diameter of 25 to 35 mm. The round rod is forged through a forging die with a hole diameter of 22 to 32 mm, finely straightened and cooled to obtain a gold alloy rod blank.
4. The method for preparing a thick-walled thin tube of electrical contact gold alloy according to claim 3, characterized in that: T 热锻 =700℃, heating time is 1.5h, and holding time is 0.5h.
5. The method for preparing a thick-walled thin tube of electrical contact gold alloy according to claim 1, characterized in that: In step three, the turning thickness of the surface oxide layer and folding is 1.0 to 1.5 mm; in step three, the centering hole after leveling and the turning to remove the surface oxide layer and folding also include cutting according to a preset length, and the preset length is 120 to 180 mm; in step four, the annealing temperature is 700°C and the annealing time is 1 hour.
6. The method for preparing a thick-walled thin tube of electrical contact gold alloy according to claim 1, characterized in that: In step five, the turning thickness is 0.5 mm; in step five, the size of the gold alloy tube blank after boring is: outer diameter 18-28 mm, inner diameter 10-15 mm, length 120-180 mm.
7. The method for preparing a thick-walled thin tube of electrical contact gold alloy according to claim 1, characterized in that: Step six specifically includes: using spring steel as a core rod, transformer oil as a lubricating oil, and a copper pipe as a push rod, and performing rotary forging with an outer diameter reduced by 2 mm per pass and a wall thickness reduced by 0.5 to 0.6 mm per pass to obtain a rotary forged pipe with an outer diameter of 12 to 14 mm and an inner diameter of 7 to 8 mm.
8. The method for preparing a thick-walled thin tube of electrical contact gold alloy according to claim 1, characterized in that: In step seven, the intermediate annealing temperature is 650°C and the time is 1h; in step seven, during the cold rolling process, the outer diameter is reduced by 1.3-2.0mm per pass, and the wall thickness is reduced by 0.2-0.5mm per pass; in step seven, the size of the pipe after the cold rolling process is: outer diameter 5.0-5.5mm, inner diameter 3.0-4.0mm.
9. The method for preparing a thick-walled thin tube of electrical contact gold alloy according to claim 1, characterized in that: In step eight, the heating annealing treatment temperature is 650°C and the time is 1h; in step eight, during the cold drawing process, the outer diameter is reduced by 1.0-1.5mm per pass, and the wall thickness is reduced by 0.1-0.15mm per pass; in step eight, the size of the tube after cold drawing is: outer diameter 2.5-4.0mm, inner diameter 1.2-2.0mm.
10. The method for preparing a thick-walled thin tube of electrical contact gold alloy according to claim 1, characterized in that: In step nine, the vacuum annealing temperature is 320° C. and the heating time is 1 h.
Citation Information
Patent Citations
Technology for preparing small-bore and thick-wall metal tubes by rotary swaging technique
CN104475479A
Preparation method of precious metal seamless tube
CN107838220A
Method of preparing titanium alloy capillary tubular product
CN108637033A
Add plug auxiliary device that swages
CN206981683U