Efficient milling cutter for machining titanium alloy
Through material selection and forging and heat treatment, and coating processing is carried out on the milling cutter, the problem of insufficient structural stability and wear resistance of the milling cutter is solved, the hardness and service life of the milling cutter is improved, and the further development is achieved. Efficient processing accuracy and reduce production costs.
Patent Information
- Application Number
- CN202411337283.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-08
AI Technical Summary
The structural stability of existing milling cutters is poor, prone to fracture and local collapse, insufficient hardness and wear resistance, resulting in reduced processing accuracy and frequent replacement, increasing consumption cost and production time.
The grain size is uniformized by material selection forging and heat treatment steps, and the hardness and wear resistance of the milling cutter are improved through coating processing, ensuring sharpness and life under high-speed cutting conditions.
It improves the structural stability and hardness of the milling cutter, extends the service life, reduces the tool replacement frequency and production cost, and ensures machining accuracy and efficiency.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of titanium alloy milling cutter processing, in particular to a high-efficiency milling cutter for processing titanium alloy. Background Art
[0002] A milling cutter is a rotating tool with one or more teeth, which is mainly used for processing planes, steps, grooves, forming surfaces and cutting off workpieces on milling machines.
[0003] A method for making a milling cutter with publication number CN108098282A comprises the following steps:
[0004] Step 1: passivation treatment, passivating the tool blank through a tool passivation machine until the surface roughness of the blank reaches 0.05-0.1um, the surface state of the tool is a glossy surface, and the direction of the processing marks cannot be distinguished, thereby obtaining a preliminary blank; Step 2: sharpening treatment, selecting a suitable grinding wheel according to the material of the tool blank and installing it in the sharpening machine, and installing the preliminary blank obtained in step 1 in the fixture of the sharpening machine for overall grooving, external cylindrical fine grinding and end face tooth gap grinding. During the above processing, the blade band of the milling cutter is reserved to obtain a finished milling cutter; before processing the cutting part, the surface of the rough blank is uniformly passivated. Due to the lack of influence of other groove structures, compared with the traditional process of first processing and then passivation, the burr removal effect on the surface of the rough blank is better during the passivation process, which reduces the scrap rate of the tool during the passivation process, and the service life of the tools in the same batch is uniform.
[0005] The above-mentioned method for manufacturing a milling cutter has an uneven grain size distribution in the structure itself, resulting in poor structural stability of the milling cutter itself. It is prone to breakage and local chipping during use, and the hardness and wear resistance of the milling cutter need to be improved. During subsequent use, the cutting surface is prone to wear and the machining accuracy is reduced, and frequent replacement is required, which increases the consumption cost of the tool and affects the machining efficiency. Summary of the invention
[0006] The purpose of the present invention is to provide a high-efficiency milling cutter for machining titanium alloys to solve the problems raised in the above-mentioned background technology.
[0007] To achieve the above object, the present invention provides the following technical solution: a high-efficiency milling cutter for processing titanium alloy, comprising the following processing steps:
[0008] Step 1: Material selection and forging: Select suitable titanium alloy raw materials and perform forging processing on them;
[0009] Step 2, mechanical processing: the titanium alloy raw material after forging in step 1 is cut into a plurality of cylindrical raw materials, and then one end of the cylindrical raw material is ground by a step difference machine, and then the ground cylindrical raw material is placed on a slotting machine and slotted, and then the slotted cylindrical raw material is placed on a fishtail machine and the blade of the milling cutter is processed to form a semi-finished milling cutter;
[0010] Step 3: Heat treatment: Place the semi-finished milling cutter in a heat treatment furnace for heat treatment, and then the formed milling cutter can be obtained;
[0011] Step 4: Appearance inspection: The milling cutter formed in step 3 is inspected by visual appearance inspection equipment, and qualified products are collected and cleaned;
[0012] Step 5, coating processing: Place the qualified milling cutter in step 4 in the spraying equipment, and then spray the wear-resistant powder coating on the milling cutter, and then put the milling cutter after the wear-resistant powder spraying into the vacuum furnace for calcination. After the calcination is completed, air cool to room temperature to obtain the titanium alloy milling cutter;
[0013] Step 6, size inspection: The titanium alloy milling cutter in step 5 is inspected for size using visual appearance inspection equipment, and qualified products are collected and cleaned. After cleaning, they are packaged to obtain the titanium alloy high-efficiency milling cutter.
[0014] Preferably, the titanium alloy raw material in step 1 is GH4169 type material.
[0015] Preferably, the titanium alloy raw material in the step one is heated to 700 degrees Celsius before forging, and during forging, the titanium alloy raw material is first added to a 700 degree Celsius heating furnace for a solid solution treatment, and then a forging press is used to perform a forging process on it, and then the titanium alloy raw material is placed in a 1100 degree Celsius heating furnace for a secondary solid solution treatment, and then a forging press is used to perform a secondary forging process on it.
[0016] Preferably, the upsetting deformation amount of the titanium alloy raw material in the first forging is 40-50%, and the upsetting deformation amount of the titanium alloy raw material in the second forging is 60-70%.
[0017] Preferably, after the blade of the cylindrical raw material is processed in step 2, it is necessary to open annular cooling grooves equidistantly arranged on the cylindrical raw material to facilitate heat dissipation when the milling cutter is used subsequently.
[0018] Preferably, when the milling cutter semi-finished product in step three is heat treated, it is first heated to 500 degrees Celsius and kept warm for 25 minutes, then heated to 650 degrees Celsius and kept warm for 70 minutes, and then the steel milling cutter semi-finished product is placed in a high-temperature salt furnace at 1100 degrees Celsius and kept warm for 7 minutes, then quenched and cooled, and then tempered.
[0019] Preferably, the tempering is divided into two times, the temperature of the first tempering is controlled at 380 degrees Celsius, the time is controlled at 8 hours, and then air-cooled to room temperature, the temperature of the first tempering is controlled at 400 degrees Celsius, the time is controlled at 6 hours, and then air-cooled to room temperature.
[0020] Preferably, the milling cutter in step four and step six needs to be placed in a mesh frame when cleaning, and then the mesh frame is placed in a degreasing cleaning liquid for immersion. After the immersion is completed, the milling cutter in the mesh frame is rinsed by spraying, and then the milling cutter can be drained. On the one hand, it can prevent the oil stains on the milling cutter from causing poor adhesion of the coating, thereby ensuring the stability of the connection of the coating. On the other hand, the surface of the milling cutter is free of oil stains when it is used.
[0021] (III) Beneficial effects
[0022] Compared with the prior art, the present invention provides a high-efficiency milling cutter for machining titanium alloy, which has the following beneficial effects:
[0023] 1. The high-efficiency milling cutter for processing titanium alloy can make the grain size inside and outside the structure of the milling cutter itself tend to be uniform or reduce the grade difference through the steps of material selection, forging and heat treatment, which can improve the quality and grain size uniformity of the inside of the milling cutter, strengthen the structural stability of the milling cutter, and prevent the milling cutter from being easily broken and partially broken during subsequent use. At the same time, it can also improve the hardness of the milling cutter, making it have the advantages of high temperature resistance, wear resistance and non-deformation, which can improve the processing accuracy and efficiency, prevent the phenomenon that the cutting surface is easy to wear and the processing accuracy is reduced due to too low hardness, and improve the quality of the milling cutter.
[0024] 2. The high-efficiency milling cutter for processing titanium alloy can maintain the sharpness and life of the tool under high-speed cutting conditions through the coating processing step, thereby reducing processing interruptions caused by frequent tool replacement, maintaining a continuous and stable processing process, and can reduce the frequent replacement required due to tool wear or breakage during subsequent use, thereby reducing the consumption cost of the tool. At the same time, it reduces the downtime caused by tool replacement, and can also ensure the accuracy and surface quality of the processed products, improve the market competitiveness of the products, improve the equipment processing efficiency and reduce production costs. DETAILED DESCRIPTION
[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Embodiment 1: A high-efficiency milling cutter for processing titanium alloy, comprising the following processing steps:
[0027] Step 1, material selection and forging: Select suitable titanium alloy raw materials and perform forging processing on them. The titanium alloy raw materials in step 1 are selected as GH4169 model materials. The titanium alloy raw materials in step 1 are first heated to 700 degrees Celsius before forging, and during forging, the titanium alloy raw materials are first added to a heating furnace at 700 degrees Celsius for a solid solution treatment, and then a forging press is used to perform a forging process on them. The titanium alloy raw materials are then placed in a heating furnace at 1100 degrees Celsius for a secondary solid solution treatment, and then a forging press is used to perform a secondary forging process on them. The upsetting deformation of the titanium alloy raw materials in the first forging is 40%, and the upsetting deformation of the titanium alloy raw materials in the secondary forging is 60%;
[0028] Step 2, mechanical processing: the titanium alloy raw material after forging in step 1 is cut into a plurality of cylindrical raw materials, and then one end of the cylindrical raw material is ground by a step difference machine, and then the ground cylindrical raw material is placed on a slotting machine and slotted, and then the slotted cylindrical raw material is placed on a fishtail machine and the blade of the milling cutter is processed to form a semi-finished milling cutter. After the blade of the cylindrical raw material is processed in step 2, it is necessary to open annular cooling grooves equidistantly arranged on the cylindrical raw material;
[0029] Step 3, heat treatment: Place the semi-finished milling cutter in a heat treatment furnace for heat treatment, and then you can get a formed milling cutter. When the semi-finished milling cutter in step 3 is heat treated, first heat it to 500 degrees Celsius and keep it warm for 25 minutes, then heat it to 650 degrees Celsius and keep it warm for 70 minutes, then put the steel milling cutter semi-finished product into a high-temperature salt furnace at 1100 degrees Celsius for 7 minutes, then quench and cool it, and then temper it. The tempering is divided into two times. The temperature of the first tempering is controlled at 380 degrees Celsius, the time is controlled at 8 hours, and then air-cooled to room temperature. The temperature of the first tempering is controlled at 400 degrees Celsius, the time is controlled at 6 hours, and then air-cooled to room temperature;
[0030] Step 4: Appearance inspection: The milling cutter formed in step 3 is inspected by visual appearance inspection equipment, and qualified products are collected and cleaned;
[0031] Step 5, coating processing: Place the qualified milling cutter in step 4 in the spraying equipment, and then spray the wear-resistant powder coating on the milling cutter, and then put the milling cutter after the wear-resistant powder spraying into the vacuum furnace for calcination. After the calcination is completed, air cool to room temperature to obtain the titanium alloy milling cutter;
[0032] Step six, size inspection: use visual appearance inspection equipment to inspect the size of the titanium alloy milling cutter in step five, collect and clean the qualified products, and pack them after cleaning to obtain the titanium alloy high-efficiency milling cutter. When cleaning, the milling cutter in steps four and six needs to be placed in a mesh frame first, and then the mesh frame is placed in a degreasing cleaning liquid for soaking. After soaking, rinse the milling cutter in the mesh frame by spraying, and then drain the milling cutter.
[0033] Embodiment 2: A high-efficiency milling cutter for processing titanium alloy, comprising the following processing steps:
[0034] Step 1, material selection and forging: Select suitable titanium alloy raw materials and perform forging processing on them. The titanium alloy raw materials in step 1 are selected as GH4169 model materials. The titanium alloy raw materials in step 1 are first heated to 700 degrees Celsius before forging, and during forging, the titanium alloy raw materials are first added to a heating furnace at 700 degrees Celsius for a solid solution treatment, and then a forging press is used to perform a forging process on them. The titanium alloy raw materials are then placed in a heating furnace at 1100 degrees Celsius for a secondary solid solution treatment, and then a forging press is used to perform a secondary forging process on them. The upsetting deformation of the titanium alloy raw materials in the first forging is 45%, and the upsetting deformation of the titanium alloy raw materials in the secondary forging is 65%;
[0035] Step 2, mechanical processing: the titanium alloy raw material after forging in step 1 is cut into a plurality of cylindrical raw materials, and then one end of the cylindrical raw material is ground by a step difference machine, and then the ground cylindrical raw material is placed on a slotting machine and slotted, and then the slotted cylindrical raw material is placed on a fishtail machine and the blade of the milling cutter is processed to form a semi-finished milling cutter. After the blade of the cylindrical raw material is processed in step 2, it is necessary to open annular cooling grooves equidistantly arranged on the cylindrical raw material;
[0036] Step 3, heat treatment: Place the semi-finished milling cutter in a heat treatment furnace for heat treatment, and then you can get a formed milling cutter. When the semi-finished milling cutter in step 3 is heat treated, first heat it to 500 degrees Celsius and keep it warm for 25 minutes, then heat it to 650 degrees Celsius and keep it warm for 70 minutes, then put the steel milling cutter semi-finished product into a high-temperature salt furnace at 1100 degrees Celsius for 7 minutes, then quench and cool it, and then temper it. The tempering is divided into two times. The temperature of the first tempering is controlled at 380 degrees Celsius, the time is controlled at 8 hours, and then air-cooled to room temperature. The temperature of the first tempering is controlled at 400 degrees Celsius, the time is controlled at 6 hours, and then air-cooled to room temperature;
[0037] Step 4: Appearance inspection: The milling cutter formed in step 3 is inspected by visual appearance inspection equipment, and qualified products are collected and cleaned;
[0038] Step 5, coating processing: Place the qualified milling cutter in step 4 in the spraying equipment, and then spray the wear-resistant powder coating on the milling cutter, and then put the milling cutter after the wear-resistant powder spraying into the vacuum furnace for calcination. After the calcination is completed, air cool to room temperature to obtain the titanium alloy milling cutter;
[0039] Step six, size inspection: use visual appearance inspection equipment to inspect the size of the titanium alloy milling cutter in step five, collect and clean the qualified products, and pack them after cleaning to obtain the titanium alloy high-efficiency milling cutter. When cleaning, the milling cutter in steps four and six needs to be placed in a mesh frame first, and then the mesh frame is placed in a degreasing cleaning liquid for soaking. After soaking, rinse the milling cutter in the mesh frame by spraying, and then drain the milling cutter.
[0040] Embodiment 3: A high-efficiency milling cutter for processing titanium alloy, comprising the following processing steps:
[0041] Step 1, material selection and forging: Select suitable titanium alloy raw materials and perform forging processing on them. The titanium alloy raw materials in step 1 are selected as GH4169 model materials. The titanium alloy raw materials in step 1 are first heated to 700 degrees Celsius before forging, and during forging, the titanium alloy raw materials are first added to a 700-degree Celsius heating furnace for a solid solution treatment, and then a forging press is used to perform a forging process on them. The titanium alloy raw materials are then placed in a 1100-degree Celsius heating furnace for a secondary solid solution treatment, and then a forging press is used to perform a secondary forging process on them. The upsetting deformation of the titanium alloy raw materials in the first forging is 50%, and the upsetting deformation of the titanium alloy raw materials in the secondary forging is 70%;
[0042] Step 2, mechanical processing: the titanium alloy raw material after forging in step 1 is cut into a plurality of cylindrical raw materials, and then one end of the cylindrical raw material is ground by a step difference machine, and then the ground cylindrical raw material is placed on a slotting machine and slotted, and then the slotted cylindrical raw material is placed on a fishtail machine and the blade of the milling cutter is processed to form a semi-finished milling cutter. After the blade of the cylindrical raw material is processed in step 2, it is necessary to open annular cooling grooves equidistantly arranged on the cylindrical raw material;
[0043] Step 3, heat treatment: Place the semi-finished milling cutter in a heat treatment furnace for heat treatment, and then you can get a formed milling cutter. When the semi-finished milling cutter in step 3 is heat treated, first heat it to 500 degrees Celsius and keep it warm for 25 minutes, then heat it to 650 degrees Celsius and keep it warm for 70 minutes, then put the steel milling cutter semi-finished product into a high-temperature salt furnace at 1100 degrees Celsius for 7 minutes, then quench and cool it, and then temper it. The tempering is divided into two times. The temperature of the first tempering is controlled at 380 degrees Celsius, the time is controlled at 8 hours, and then air-cooled to room temperature. The temperature of the first tempering is controlled at 400 degrees Celsius, the time is controlled at 6 hours, and then air-cooled to room temperature;
[0044] Step 4: Appearance inspection: The milling cutter formed in step 3 is inspected by visual appearance inspection equipment, and qualified products are collected and cleaned;
[0045] Step 5, coating processing: Place the qualified milling cutter in step 4 in the spraying equipment, and then spray the wear-resistant powder coating on the milling cutter, and then put the milling cutter after the wear-resistant powder spraying into the vacuum furnace for calcination. After the calcination is completed, air cool to room temperature to obtain the titanium alloy milling cutter;
[0046] Step six, size inspection: use visual appearance inspection equipment to inspect the size of the titanium alloy milling cutter in step five, collect and clean the qualified products, and pack them after cleaning to obtain the titanium alloy high-efficiency milling cutter. When cleaning, the milling cutter in steps four and six needs to be placed in a mesh frame first, and then the mesh frame is placed in a degreasing cleaning liquid for soaking. After soaking, rinse the milling cutter in the mesh frame by spraying, and then drain the milling cutter.
[0047] It can be seen that: the grain size distribution of some milling cutter structures itself is not uniform, resulting in poor structural stability of the milling cutter itself, which is prone to breakage and local chipping during use. The high-efficiency milling cutter for processing titanium alloys, through the steps of material selection, forging and heat treatment, makes the grain size inside and outside the milling cutter structure tend to be uniform or reduce the grade difference, which can improve the quality and grain size uniformity inside the milling cutter, strengthen the structural stability of the milling cutter, and prevent the milling cutter from being prone to breakage and local chipping during subsequent use. At the same time, it can also improve the hardness of the milling cutter, making it resistant to high temperature, wear-resistant and not easy to deform, which can improve the processing accuracy and efficiency, prevent the phenomenon that the cutting surface is easy to wear and the processing accuracy is reduced due to too low hardness, and improve the quality of the milling cutter. Secondly, the milling cutter The hardness and wear resistance of the titanium alloy need to be improved. In subsequent use, the cutting surface will be easily worn and the processing accuracy will be reduced. Frequent replacement is required, which increases the consumption cost of the tool and affects the processing efficiency. The high-efficiency milling cutter for processing titanium alloy can maintain the sharpness and life of the tool under high-speed cutting conditions through the coating processing steps, thereby reducing the processing interruptions caused by frequent tool replacement and maintaining a continuous and stable processing process. In subsequent use, the frequent replacement required due to tool wear or breakage can be reduced, reducing the consumption cost of the tool. At the same time, the downtime caused by tool replacement is reduced, and the accuracy and surface quality of the processed products can be guaranteed, the market competitiveness of the products is improved, the equipment processing efficiency is improved and the production cost is reduced.
[0048] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An efficient milling cutter for machining titanium alloys. It is characterized in that The processing steps include: Step 1: Material selection and forging: Select suitable titanium alloy raw materials and perform forging processing on them; Step 2, mechanical processing: the titanium alloy raw material after forging in step 1 is cut into a plurality of cylindrical raw materials, and then one end of the cylindrical raw material is ground by a step difference machine, and then the ground cylindrical raw material is placed on a slotting machine and slotted, and then the slotted cylindrical raw material is placed on a fishtail machine and the blade of the milling cutter is processed to form a semi-finished milling cutter; Step 3: Heat treatment: Place the semi-finished milling cutter in a heat treatment furnace for heat treatment, and then the formed milling cutter can be obtained; Step 4: Appearance inspection: The milling cutter formed in step 3 is inspected by visual appearance inspection equipment, and qualified products are collected and cleaned; Step 5, coating processing: Place the qualified milling cutter in step 4 in the spraying equipment, and then spray the wear-resistant powder coating on the milling cutter, and then put the milling cutter after the wear-resistant powder spraying into the vacuum furnace for calcination. After the calcination is completed, air cool to room temperature to obtain the titanium alloy milling cutter; Step 6, size inspection: The titanium alloy milling cutter in step 5 is inspected for size using visual appearance inspection equipment, and qualified products are collected and cleaned. After cleaning, they are packaged to obtain the titanium alloy high-efficiency milling cutter.
2. A high-efficiency milling cutter for machining titanium alloy according to claim 1, Features: The titanium alloy raw material in step 1 is selected as GH4169 type material.
3. A high-efficiency milling cutter for machining titanium alloy according to claim 2, Features: The titanium alloy raw material in the step 1 is heated to 700 degrees Celsius before forging, and during forging, the titanium alloy raw material is first added to a 700 degree Celsius heating furnace for a solid solution treatment, and then a forging press is used to perform a forging process on it, and then the titanium alloy raw material is placed in a 1100 degree Celsius heating furnace for a secondary solid solution treatment, and then a forging press is used to perform a secondary forging process on it.
4. A high-efficiency milling cutter for machining titanium alloy according to claim 3, Features: The upsetting deformation amount of the titanium alloy raw material during the primary forging is 40-50%, and the upsetting deformation amount of the titanium alloy raw material during the secondary forging is 60-70%.
5. The high-efficiency milling cutter for machining titanium alloy according to claim 4, Features: After the blade of the cylindrical raw material is processed in step 2, it is necessary to open annular cooling grooves equidistantly arranged on the cylindrical raw material.
6. The high-efficiency milling cutter for machining titanium alloy according to claim 5, Features: When the semi-finished milling cutter in step three is heat treated, it is first heated to 500 degrees Celsius and kept warm for 25 minutes, then heated to 650 degrees Celsius and kept warm for 70 minutes, and then the semi-finished steel milling cutter is placed in a high-temperature salt furnace at 1100 degrees Celsius and kept warm for 7 minutes, then quenched and cooled, and then tempered.
7. The high-efficiency milling cutter for machining titanium alloy according to claim 6, Features: The tempering is divided into two times. The temperature of the first tempering is controlled at 380 degrees Celsius, the time is controlled at 8 hours, and then it is air-cooled to room temperature. The temperature of the first tempering is controlled at 400 degrees Celsius, the time is controlled at 6 hours, and then it is air-cooled to room temperature.
8. The high-efficiency milling cutter for machining titanium alloy according to claim 7, Features: When cleaning the milling cutter in step 4 and step 6, it is necessary to first place it in a mesh frame, and then place the mesh frame in a degreasing cleaning solution for soaking. After soaking, rinse the milling cutter in the mesh frame by spraying, and then drain the milling cutter.
Citation Information
Patent Citations
Forging technology for high-strength and abrasion-resisting milling tool
CN109333015A
Machining method of high-precision speed reducer gland
CN110227907A
Forging process for high-strength wear-resistant milling cutter
CN111074168A
Preparation process of hard alloy milling cutter
CN112756929A