Production method of criss-cross ultrathin high-softness bamboo composite board

By using water-based polyurethane adhesives and a drying process for non-woven fabrics, the warping and deformation problem caused by moisture absorption in ultra-thin bamboo composite boards has been solved, improving the stability and aesthetics of the boards. This makes them suitable for special applications such as decoration and packaging materials, and aligns with the trend of green consumption.

CN118906157AInactive Publication Date: 2024-11-08ZHEJIANG XINGSHANG SMART HOME CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411155041.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional ultra-thin bamboo composite boards absorb moisture rapidly after being bonded with water-containing adhesives, resulting in a significant increase in moisture content. This causes uneven shrinkage of the boards along the radial direction, leading to severe warping and deformation.

Method used

Water-based polyurethane adhesive and non-woven fabric are used as auxiliary materials. The high-temperature and high-pressure drying process ensures that the moisture content of the composite material is consistent. Combined with chemical fiber non-woven fabric as a carrier, moisture absorption is avoided. The dry-in and dry-out process ensures the stability of the board.

Benefits of technology

It effectively avoids warping and deformation, improves the structural stability and aesthetics of the board, meets consumer needs, is suitable for special scenarios, and is environmentally friendly and energy-saving, simplifying the production process.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of composite boards, in particular to a production method of a criss-cross ultrathin high-softness bamboo composite board, which comprises the following steps: preparation of micro thin bamboo chips, material preparation, gluing process, preliminary drying, structure assembly and pressing, post-treatment and finished product inspection. Wherein for primary drying, the non-woven fabric coated with glue is tightly attached to the thin bamboo chips, and the thin bamboo chips are placed in a multi-layer hot press to be subjected to primary drying treatment; and for structure assembling and pressing, after being transversely cut off, the micro thin bamboo chips are placed on the non-woven fabric of the product obtained through preliminary drying to form a structure of an upper-layer transverse thin bamboo, a middle non-woven fabric and a lower-layer forward thin bamboo, and then the three layers of objects are placed into a hot press together to be pressed under the high-temperature and high-pressure condition. The structural stability and attractiveness of the bamboo composite board are improved, environmental friendliness, ultra-thin softness, production efficiency and cost optimization are also considered, and the bamboo composite board is wide in application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite boards, in particular to a production method of a crisscrossed ultra-thin high-softness bamboo composite board. Background Art

[0002] The design of traditional bamboo or bamboo-wood composite materials emphasizes the configuration of the base layers and the symmetry of the structure, aiming to effectively cope with the fluctuations in the moisture content of the board caused by changes in environmental humidity, thereby reducing the risk of warping and deformation of the board.

[0003] However, if the product uses an ultra-thin structure with two layers (each layer is only 0.3mm), a new problem will arise: if water-containing adhesives are used directly for compounding, the water will be easily absorbed by the extremely thin board quickly, causing the moisture content of the board to increase significantly by 3-5%. In the subsequent drying environment, the evaporation of this excess water will cause the board to shrink significantly in the radial direction. Since the fiber directions of the upper and lower layers of the board are staggered, the shrinkage directions are inconsistent, thus inducing serious warping and deformation problems.

[0004] Therefore, in view of this situation, it is urgent to develop a production method for criss-crossed ultra-thin and highly flexible bamboo composite panels to overcome the shortcomings in current practical applications. Summary of the invention

[0005] The purpose of the embodiments of the present invention is to provide a method for producing a criss-crossed ultra-thin high-flexibility bamboo composite board to solve the problems raised in the above-mentioned background technology.

[0006] To achieve the above objectives, the embodiments of the present invention provide the following technical solutions:

[0007] A method for producing a crisscrossed ultra-thin high-softness bamboo composite board comprises the following steps:

[0008] Step 1: Preparation of thin bamboo slices

[0009] The thin bamboo slices with a thickness of 0.3 mm are obtained by slicing technology, and then dried to control the moisture content at 9-12%, and then selected for use;

[0010] Step 2: Material preparation

[0011] Select water-based polyurethane adhesive and non-woven fabric as auxiliary materials for standby use;

[0012] Step 3: Gluing process

[0013] Use three-roll or four-roll gluing equipment to evenly apply water-based polyurethane adhesive on both sides of the non-woven fabric, ensuring that the coating amount on each side is 60-70g / m 2 ;

[0014] Step 4: Preliminary drying

[0015] The non-woven fabric coated with glue is tightly attached to the thin bamboo slices obtained in step 1, and placed in a multi-layer hot press for preliminary drying, so that the moisture content of the composite material is stabilized at 8-12%;

[0016] Step 5: Structural assembly and pressing

[0017] Cut the thin bamboo slices obtained in step 1 transversely and place them on the non-woven fabric of the product obtained in step 4 to form a structure of an upper transverse thin bamboo, a middle non-woven fabric, and a lower longitudinal thin bamboo. Then put the three layers of articles into a hot press and press them under high temperature and high pressure conditions.

[0018] Step 6: Post-processing and finished product inspection

[0019] After the pressing is completed, the product is removed from the hot press for heat dissipation and left to stand naturally to stabilize the structure; then it is repaired, sanded, and cut, and the finished product is obtained after passing the quality inspection.

[0020] As a further solution of the present invention: in step 2, the water-based polyurethane adhesive is mainly composed of water-based PUD, PA, and EVA, and has a solid content of 40-50%.

[0021] As a further solution of the present invention: in step 2, the specification of the non-woven fabric is 20-25 g / m 2 It is made by needle-punched hot-rolling process. Its main components are a mixture of one or more of polyester, polypropylene, nylon, spandex and acrylic. Its color is khaki or khaki.

[0022] As a further solution of the present invention: iron oxide yellow and iron oxide brown pigments are also added to the water-based polyurethane adhesive.

[0023] As a further solution of the present invention: in step 4, the temperature of the hot press is set to 80-110° C., and the hot press is kept turned on after the non-woven fabric and the thin bamboo slices are placed in.

[0024] As a further solution of the present invention: in step 5, the hot pressing temperature is controlled at 120-140°C, the holding time is 50-100 seconds, and the pressure is maintained at 10-15 kg / cm2.

[0025] As a further solution of the present invention: in step 6, the natural standing time shall not be less than 48 hours.

[0026] Compared with the prior art, the embodiments of the present invention have the following beneficial effects:

[0027] 1) By introducing water-based polyurethane adhesive and combining chemical fiber non-woven fabric as a carrier, the problem of warping caused by moisture content changes caused by the board directly absorbing moisture from the glue in the traditional process is effectively avoided. This dry-in and dry-out high-temperature pressing process ensures that the moisture content of the upper and lower layers of the board is consistent, greatly reducing the risk of asymmetric deformation and significantly improving the structural stability of the composite board.

[0028] 2) Due to the stable structure, the surface of the board is smoother, without warping or deformation, which improves the overall aesthetics of the product and meets consumers' demand for high-quality products.

[0029] 3) The total thickness of the product does not exceed 0.6mm, while maintaining extremely high softness, making it suitable for more special scenarios, such as decorative materials and packaging materials that require ultra-thin and flexible materials.

[0030] 4) The use of formaldehyde-free glue (water-based polyurethane adhesive) reduces the release of harmful substances, is environmentally friendly, and conforms to the trend of modern green consumption.

[0031] 5) There is no need to use special equipment for gluing and drying non-woven fabrics, which simplifies the production process, saves site space, reduces equipment investment, and reduces energy consumption and costs in the production process, thereby improving overall production efficiency.

[0032] 6) Because the product is ultra-thin and soft, it has a stronger ability to adapt to different usage environments, especially when the moisture content of the board is basically consistent with the usage environment, it can maintain extremely high flatness and stability. DETAILED DESCRIPTION

[0033] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] An embodiment of the present invention provides a method for producing a criss-crossed ultra-thin high-flexibility bamboo composite board, comprising the following steps:

[0035] Step 1: Preparation of thin bamboo slices

[0036] The planing technology is used to obtain thin bamboo slices with a thickness of 0.3mm, which are then dried and the moisture content is controlled at 9-12%. They are selected and set aside.

[0037] Step 2: Material preparation

[0038] Select water-based polyurethane adhesive and non-woven fabric of specific specifications as auxiliary materials and set them aside.

[0039] Step 3: Gluing process

[0040] Use three-roll or four-roll gluing equipment to evenly apply water-based polyurethane adhesive on both sides of the non-woven fabric, ensuring that the coating amount on each side is 60-70g / m 2 , for best bonding effect.

[0041] Step 4: Preliminary drying

[0042] The glue-coated nonwoven fabric is tightly attached to the thin bamboo slices obtained in step 1, and placed in a multi-layer hot press for preliminary drying. The drying conditions are strictly controlled to stabilize the moisture content of the composite material at 8-12%.

[0043] Step 5: Structural assembly and pressing

[0044] The thin bamboo slices obtained in step 1 are cut transversely and placed on the non-woven fabric of the product obtained in step 4 to form a structure of an upper transverse thin bamboo layer, a middle non-woven fabric, and a lower longitudinal thin bamboo layer. The three layers are then put into a hot press together and pressed under high temperature and high pressure conditions to ensure that the layers are tightly bonded.

[0045] Step 6: Post-processing and finished product inspection

[0046] After the pressing is completed, the product is quickly removed from the hot press for heat dissipation and left to stand naturally to stabilize the structure. Then, post-processing procedures such as repairing, sanding, and cutting are carried out, and finally, strict quality inspection is carried out to ensure that the quality of the finished product meets the standards.

[0047] Among them, in step 2, the water-based polyurethane adhesive used is a special formula, mainly composed of water-based PUD, PA, EVA, etc., with a solid content of 40-50%, high molecular weight, low viscosity and excellent drying film-forming and secondary high-temperature bonding properties. The film is soft and bright, with strong bonding force, and is widely used in the bonding of various materials such as wood, plastic, leather, etc.

[0048] In step 2, non-woven fabric is used as an adhesive carrier with a specification of 20-25 g / m 2 It is made of needle-punched hot-rolled technology. Its main components are a mixture of one or more of polyester, polypropylene, nylon, spandex and acrylic. The color is mainly khaki or khaki, which complements the color of the thin bamboo slices.

[0049] Preferably, iron oxide yellow and iron oxide brown pigments are added to the water-based polyurethane adhesive and mixed to a color close to that of the thin bamboo slices to enhance the overall aesthetics of the product.

[0050] In step 4, the initial drying stage, the temperature of the heat press is set to 80-110°C, and the heat press is kept on after the items (non-woven fabrics and thin bamboo pieces) are placed in to ensure the drying effect and material safety.

[0051] In step 5, during the pressing stage, the hot pressing temperature is controlled at 120-140°C, the holding time is 50-100 seconds, and the pressure is maintained at 10-15kg / cm2 to ensure the pressing quality of the product.

[0052] In step 6, the natural standing time must not be less than 48 hours to ensure that the internal stress of the product is fully released and the structure is more stable.

[0053] The above-mentioned embodiment of the present invention provides a method for producing a criss-cross ultra-thin and highly flexible bamboo composite board, which introduces a water-based polyurethane adhesive and combines a chemical fiber non-woven fabric as a carrier of the adhesive. In the specific operation, the water-based polyurethane adhesive is first evenly coated on the non-woven fabric, and then the composite layer is placed on a single layer of thin bamboo for drying to completely remove the moisture in the adhesive. This method not only effectively avoids the direct absorption of moisture by the board, but also ensures a dry environment during the composite process, thereby significantly reducing the risk of warping and deformation of the board due to changes in moisture content (the process of high-temperature pressing of materials with dry in and dry out is adopted to avoid the problem of asymmetric deformation of the upper and lower layers of thin bamboo in the finished product due to changes in moisture content after the thin bamboo absorbs moisture in the adhesive after pressing with traditional glue), achieving a double improvement in the structural stability and aesthetics of the composite board.

[0054] In addition, the total thickness of the product does not exceed 0.6mm. When the moisture content is basically consistent with the use environment, it is particularly flat and soft, meeting the needs of consumers in special scenarios. It uses formaldehyde-free glue, which is environmentally friendly. There is no need to use special equipment for gluing and drying non-woven fabrics, which saves space, saves investment, and reduces production costs.

[0055] The above are only preferred embodiments of the present invention. It should be pointed out that, for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present invention. These should also be regarded as the protection scope of the present invention. These will not affect the effect of the implementation of the present invention and the practicality of the patent.

Claims

1. A method for producing a crisscross ultra-thin high-softness bamboo composite board, characterized in that: The following steps are involved: Step 1: Preparation of thin bamboo slices The thin bamboo slices with a thickness of 0.3 mm are obtained by slicing technology, and then dried to control the moisture content at 9-12%, and then selected for use; Step 2: Material preparation Select water-based polyurethane adhesive and non-woven fabric as auxiliary materials for standby use; Step 3: Gluing process Use three-roll or four-roll gluing equipment to evenly apply water-based polyurethane adhesive on both sides of the non-woven fabric, ensuring that the coating amount on each side is 60-70g / m 2 ; Step 4: Preliminary drying The non-woven fabric coated with glue is tightly attached to the thin bamboo slices obtained in step 1, and placed in a multi-layer hot press for preliminary drying, so that the moisture content of the composite material is stabilized at 8-12%; Step 5: Structural assembly and pressing Cut the thin bamboo slices obtained in step 1 transversely and place them on the non-woven fabric of the product obtained in step 4 to form a structure of an upper transverse thin bamboo, a middle non-woven fabric, and a lower longitudinal thin bamboo. Then put the three layers of articles into a hot press and press them under high temperature and high pressure conditions. Step 6: Post-processing and finished product inspection After the pressing is completed, the product is removed from the hot press for heat dissipation and left to stand naturally to stabilize the structure; then it is repaired, sanded, and cut, and the finished product is obtained after passing the quality inspection.

2. The method for producing the criss-crossed ultra-thin high-flexibility bamboo composite board according to claim 1, characterized in that: In step 2, the water-based polyurethane adhesive is mainly composed of water-based PUD, PA, and EVA, and the solid content is 40-50%.

3. The method for producing the crisscross ultra-thin high-flexibility bamboo composite board according to claim 2, characterized in that: In step 2, the specification of non-woven fabric is 20-25g / m 2 It is made by needle-punched hot-rolling process. Its main components are a mixture of one or more of polyester, polypropylene, nylon, spandex and acrylic. Its color is khaki or khaki.

4. The method for producing the crisscross ultra-thin high-flexibility bamboo composite board according to claim 2, characterized in that: Iron oxide yellow and iron oxide brown pigments are also added to the water-based polyurethane adhesive.

5. The method for producing a crisscrossed ultra-thin high-flexibility bamboo composite board according to any one of claims 1 to 4, characterized in that: In step 4, the temperature of the hot press is set to 80-110° C., and the hot press is kept turned on after the non-woven fabric and the thin bamboo slices are placed in.

6. The method for producing the crisscross ultra-thin high-flexibility bamboo composite board according to claim 5, characterized in that: In step 5, the hot pressing temperature is controlled at 120-140°C, the holding time is 50-100 seconds, and the pressure is maintained at 10-15 kg / cm2.

7. The method for producing the crisscross ultra-thin high-flexibility bamboo composite board according to claim 1, characterized in that: In step 6, the natural standing time shall not be less than 48 hours.

Citation Information

Patent Citations

  • Wood floor manufacturing method

    CN105089248A

  • Method for preparing decorative veneer from sliced thin bamboos

    CN105666988A

  • Bamboo and rattan woven surface decorative plate and manufacturing method thereof

    CN116604895A

  • Ultra-thin fiberboard-based decorative structure

    CN219749103U

  • Composite decoration bamboo material

    CN2544924Y