Preparation method of durable termite-proof wood

By opening holes in the wood and using impregnation of anti-termite agents and silicon sols combined with wood fillers and reinforcers, the problems of coating damage and reduction in prevention and treatment effects in existing anti-termite treatment methods are solved, and long-lasting anti-termite and anti-corrosion are achieved Antibacterial effect.

CN118906164APending Publication Date: 2024-11-08BEIJING FORESTRY UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410961325.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing anti-termite wood treatment methods such as spraying and spraying methods have problems such as coating damage and the reduction in the prevention and control effect over time, making it difficult to achieve a lasting anti-termite effect.

Method used

Drilling equipment is used to open holes at certain intervals on the wood, and use a mixture of anti-termite agent and silicon sol for pressurized impregnation, combined with wood filler and reinforcement, and then apply anticorrosion paint to form a multi-layer protection effect.

Benefits of technology

By strengthening the impregnation effect of wood and filling holes, the anti-corrosion and anti-bacterial ability of wood is enhanced, the anti-termite effect is extended, and the cracking of holes is prevented, achieving the purpose of long-lasting termite prevention.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of wood processing treatment, and discloses a preparation method of durable termite-proof wood, which comprises the following specific steps: step 1, preparing a wood raw material with a good condition, and then cutting the wood raw material into wood raw material sections with the same length by using a cutting machine; and secondly, drilling equipment is used for conducting hole forming operation on the specification wood according to a certain interval. According to the method, through the mode of combining impregnation of the wood impregnation stock solution on the specification wood and brushing of the wood anti-corrosion paint on the outer surface of the specification wood, the anti-corrosion capacity of the outer surface of the specification wood is enhanced while termites of the specification wood are prevented, so that natural volatilization of the wood impregnation stock solution is slowed down, and then the purpose of lasting prevention of the termites is achieved; and the dipping effect of the wood can be enhanced by forming the holes in the specification wood at equal intervals, the strength of the specification wood is enhanced with the assistance of the wood filling agent and the wood reinforcing agent, and the situation that the wood cracks in the subsequent use process due to the holes is prevented.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of wood processing and treatment, and specifically relates to a method for preparing durable termite-proof wood. Background Art

[0002] Termites are insects of the family Termitidae in the order Isoptera. They are small in size and are named termites because of their grayish-white body color. They are distributed in tropical and subtropical regions and live in warm, humid, and secluded places. They mainly feed on cellulose and hemicellulose from plants and wood, such as plant roots, stems and bark, wood, dry branches and fallen leaves, and wood processing products containing cellulose. They cause severe damage to buildings, especially brick-wood and wooden structures.

[0003] When constructing brick-wood structure houses, etc., corresponding measures need to be taken to prevent and control termites, so as to prevent termites from hiding inside the wood structure, destroying or damaging its bearing points, causing the house to collapse suddenly, etc., and the existing measures generally involve anti-corrosion treatment of building wood, but the existing anti-termite wood often only uses a single spraying method or a spray immersion method to treat the wood. Both of these treatment methods have disadvantages. When the surface coating of the wood treated by the spraying method is damaged, it is still susceptible to corrosion by termites. Although the spray immersion method can prevent and control termites, its prevention and control effect will decrease over time with the erosion of the natural environment and the volatilization of the impregnation agent, so it is necessary to improve this. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a method for preparing durable termite-proof wood, which has the advantage of durable termite-proofing.

[0005] To achieve the above object, the present invention provides the following technical solution: a method for preparing durable termite-proof wood, the specific steps are as follows:

[0006] Step 1:

[0007] Prepare good-quality wood materials, then use a cutting machine to split the wood materials into wood material segments of equal length, and then use a cutting device to cut the wood material segments, peel the wood material segments and cut them into wood of the same size;

[0008] Step 2:

[0009] Use drilling equipment to drill holes in the standard wood at certain intervals, then clean the drilled standard wood and remove sawdust and dust from the wood surface and holes;

[0010] Step 2:

[0011] Prepare anti-termite agent and silica sol, mix them in a ratio of 1:5, add them into a mixing tank and stir them thoroughly for 30 minutes to one hour, so that the anti-termite agent and silica sol are fully mixed to form a wood impregnation stock solution;

[0012] Step 3:

[0013] Put the treated standard wood into a pressure tank, then add the wood impregnation solution, and pressurize and impregnate for ten hours at 60 degrees Celsius and 1Mpa atmospheric pressure to make the wood impregnation solution fully penetrate into the standard wood. At this time, under the action of silica sol, the anti-termite agent will be firmly adsorbed on the inner layer of the standard wood. Then, vacuum pumping operation is performed to drain the excess solution in the pressure tank and take out the standard wood;

[0014] Step 4:

[0015] Put the impregnated standard wood into the drying box, then adjust the temperature to 80 degrees Celsius for drying. After 10 hours, take out the standard wood and cool it naturally to room temperature to dry out the excess moisture in the standard wood. Then test the moisture content inside the wood. If the moisture content is below 15%, you can continue the subsequent operation. If the moisture content is still over 15%, put the standard wood back into the drying box to continue the drying operation. Then use the fan to clean the dust attached to the outer surface of the cooled standard wood and the residual debris in the holes for a second time. After cleaning, prepare two parts of filler and one part of adhesive. , put them into a mixing barrel and stir and mix them in a ratio of 2:1 to make a wood filler, then put the wood filler into a vibration device for vibration treatment and take it out after thirty minutes, observe whether there are still bubbles inside the wood filler, if there are still bubbles, continue to use the vibration device to treat until the bubbles inside the wood filler are completely removed, and obtain a filling agent that meets the standards, and finally inject the prepared wood filler into the holes opened in the standard wood at room temperature, and then let it stand for 24 hours to allow the wood filler and the inner wall of the hole opened on the standard wood to fully adhere to each other, so as to fill the hole;

[0016] Step 5:

[0017] Use grinding equipment to carefully grind the filled standard wood to remove excess wood filler and bumps on the wood surface to make the surface of the standard wood smooth. After grinding, use vacuum equipment to clean up the debris and dust on the outer surface of the standard wood. Then, evenly apply a layer of wood enhancer on the surface of the standard wood to reinforce the standard wood to prevent the standard wood from cracking during subsequent use due to the opening of holes.

[0018] Step 6:

[0019] Pour the wood anticorrosive paint into a mixing bucket, stir evenly, add 0-20% clean water to dilute, and then stir thoroughly again to obtain the wood anticorrosive paint stock solution. Subsequently, a layer of the wood anticorrosive paint stock solution is evenly applied on the outer surface of the standard wood and placed in a well-ventilated place for natural ventilation. After 4 hours, a layer of the wood anticorrosive paint stock solution is applied again, and after ventilation and drying, the preparation of the durable termite-proof wood is completed.

[0020] Preferably, the certain intervals described in step 2 can be drilled at intervals of 10 cm or 20 cm according to the size of the standard wood, and the depth of the holes can be selected to be fully penetrated or half-penetrated according to the thickness of the standard wood.

[0021] Preferably, the anti-termite agent described in step three is made of 5% concentration of sulfluramid reagent, which is an organic fluorine termiticide.

[0022] Preferably, the silica sol described in step three will be dehydrated to generate silicon dioxide after being heated, and silicon dioxide has a high specific surface area and can effectively absorb the anti-termite agent and fill the interior of the wood.

[0023] Preferably, during the drying process of the standard wood in step 4, it is necessary to ensure that the standard wood maintains a constant weight after drying.

[0024] Preferably, the filler in step 4 is made of calcium stearate, which is a naturally curable inorganic filler that can fill cracks and holes on the surface of wood.

[0025] Preferably, the adhesive in step 4 is made of polyurethane, which is a commonly used adhesive having good filling and bonding properties when filling cracks and holes on the surface of wood.

[0026] Preferably, the wood enhancer described in step five mainly includes modified polyurethane and active enzyme preparations, which are used to improve the hardness, strength, weather resistance, corrosion resistance, moisture resistance and waterproofness of standard wood, and to seal the unpleasant odors such as grease inside the wood, and the infiltration and volatilization of chemical substances such as formaldehyde.

[0027] Preferably, the wood anticorrosive paint described in step six adopts Mugunghwa water-based wood anticorrosive paint, which has high antibacterial activity, can inhibit the corrosion and damage of various bacteria, molds, fungi, etc. to wood fibers, and can form a protective paint film on the wood surface.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] The present invention combines the impregnation of standard wood with wood impregnation liquid and the brushing of wood anticorrosive paint on the outer surface of standard wood, so that the standard wood can prevent and control termites while enhancing the anti-corrosion ability of the outer surface of the standard wood, thereby slowing down the natural volatilization of the wood impregnation liquid, and further achieving the purpose of long-term prevention of termites. The method of opening holes at equal intervals in the standard wood can enhance the impregnation effect of the wood, and supplemented by wood fillers and wood strengtheners to enhance the strength of the standard wood, thereby preventing the holes from causing the wood to crack during subsequent use. DETAILED DESCRIPTION

[0030] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.

[0031] The present invention provides a technical solution: a method for preparing durable termite-proof wood, the specific steps are as follows:

[0032] Step 1:

[0033] Prepare good-quality wood materials, then use a cutting machine to split the wood materials into wood material segments of equal length, and then use a cutting device to cut the wood material segments, peel the wood material segments and cut them into wood of the same size;

[0034] Step 2:

[0035] Use drilling equipment to drill holes in the standard wood at certain intervals, then clean the drilled standard wood and remove sawdust and dust from the wood surface and holes;

[0036] Step 2:

[0037] Prepare anti-termite agent and silica sol, mix them in a ratio of 1:5, add them into a mixing tank and stir them thoroughly for 30 minutes to one hour, so that the anti-termite agent and silica sol are fully mixed to form a wood impregnation stock solution;

[0038] Step 3:

[0039] Put the treated standard wood into a pressure tank, then add the wood impregnation solution, and pressurize and impregnate for ten hours at 60 degrees Celsius and 1Mpa atmospheric pressure to make the wood impregnation solution fully penetrate into the standard wood. At this time, under the action of silica sol, the anti-termite agent will be firmly adsorbed on the inner layer of the standard wood. Then, vacuum pumping operation is performed to drain the excess solution in the pressure tank and take out the standard wood;

[0040] Step 4:

[0041] Put the impregnated standard wood into the drying box, then adjust the temperature to 80 degrees Celsius for drying. After 10 hours, take out the standard wood and cool it naturally to room temperature to dry out the excess moisture in the standard wood. Then test the moisture content inside the wood. If the moisture content is below 15%, you can continue the subsequent operation. If the moisture content is still over 15%, put the standard wood back into the drying box to continue the drying operation. Then use the fan to clean the dust attached to the outer surface of the cooled standard wood and the residual debris in the holes for a second time. After cleaning, prepare two parts of filler and one part of adhesive. , put them into a mixing barrel and stir and mix them in a ratio of 2:1 to make a wood filler, then put the wood filler into a vibration device for vibration treatment and take it out after thirty minutes, observe whether there are still bubbles inside the wood filler, if there are still bubbles, continue to use the vibration device to treat until the bubbles inside the wood filler are completely removed, and obtain a filling agent that meets the standards, and finally inject the prepared wood filler into the holes opened in the standard wood at room temperature, and then let it stand for 24 hours to allow the wood filler and the inner wall of the hole opened on the standard wood to fully adhere to each other, so as to fill the hole;

[0042] Step 5:

[0043] Use grinding equipment to carefully grind the filled standard wood to remove excess wood filler and bumps on the wood surface to make the surface of the standard wood smooth. After grinding, use vacuum equipment to clean up the debris and dust on the outer surface of the standard wood. Then, evenly apply a layer of wood enhancer on the surface of the standard wood to reinforce the standard wood to prevent the standard wood from cracking during subsequent use due to the opening of holes.

[0044] Step 6:

[0045] Pour the wood anticorrosive paint into a mixing bucket, stir evenly, add 0-20% clean water to dilute, and then stir thoroughly again to obtain the wood anticorrosive paint stock solution. Subsequently, a layer of the wood anticorrosive paint stock solution is evenly applied on the outer surface of the standard wood and placed in a well-ventilated place for natural ventilation. After 4 hours, a layer of the wood anticorrosive paint stock solution is applied again, and after ventilation and drying, the preparation of the durable termite-proof wood is completed.

[0046] The present invention strengthens the impregnation effect of the wood impregnation solution by pre-drilling holes in the standard wood, so that the standard wood is more fully impregnated, and the holes opened can be filled with a wood filler, and a layer of wood reinforcing agent is applied to the outer surface of the standard wood to prevent the standard wood from cracking at the holes during subsequent use, thereby enhancing the strength of the standard wood. Finally, the wood anti-corrosion paint applied is combined with the impregnation of the wood impregnation solution, so that the standard wood has a long-lasting anti-termite effect and enhances the anti-corrosion and antibacterial ability of the standard wood.

[0047] The certain intervals in step 2 can be made at intervals of 10 cm or 20 cm according to the size of the standard wood, and the depth of the holes can be selected to be fully penetrated or half-penetrated according to the thickness of the standard wood.

[0048] The holes opened on the sized wood should be uniform, so as to improve the impregnation efficiency and quality of the wood impregnation solution.

[0049] The anti-termite agent in step three is made of 5% concentration of sulfluramid reagent, which is an organic fluorine termiticide.

[0050] Sulfluramid can inhibit the energy metabolism of termites, prevent energy conversion, slow down the insects' heart rate, hinder their respiratory movements, and reduce their oxygen consumption, thereby effectively preventing and controlling termites and reducing their gnawing on standard wood.

[0051] Among them, the silica sol in step three will be dehydrated to form silicon dioxide after heating. Silicon dioxide has a high specific surface area and can effectively absorb anti-termite agents and fill the interior of the wood.

[0052] Silica sol is a dispersion of nano-scale silicon dioxide particles in water or solvent. It is odorless, non-toxic, and has the characteristics of strong adhesion and high temperature resistance. It is also resistant to pollution, dust, aging, and fire. When adding anti-termite agents to silica sol, ethanol can be added to increase the mixing degree of the anti-termite agent and silica sol.

[0053] During the drying process of the standard wood in step 4, it is necessary to ensure that the standard wood maintains a constant weight after drying.

[0054] By drying the moisture inside the standard wood, the anti-corrosion effect of the wood can be further improved and the corrosion resistance of the wood can be improved.

[0055] The filler in step 4 is made of calcium stearate, which is a naturally curable inorganic filler that can fill cracks and holes on the surface of wood.

[0056] During the filling process, calcium stearate forms a hard coating on the wood surface, which can effectively protect the wood from wear and decay.

[0057] Among them, the adhesive in step four is made of polyurethane, which is a commonly used adhesive and has good filling and bonding properties when filling cracks and holes on the surface of wood.

[0058] Polyurethane can cure into a hard structure to protect the wood surface from damage and aging. When mixed with calcium stearate filler in a ratio of 1:2, it can effectively fill the holes opened in standard wood.

[0059] Among them, the wood enhancer in step five mainly includes modified polyurethane and active enzyme preparations, which are used to improve the hardness, strength, weather resistance, corrosion resistance, moisture resistance and waterproofness of standard wood, and to seal the unpleasant odors such as grease inside the wood, and the infiltration and volatilization of chemicals such as formaldehyde.

[0060] Modified polyurethane is a two-component characteristic material with the characteristics of environmental protection, high closure, high toughness and high hardness. It can stabilize the moisture content of wood and prevent deformation and cracking. Active enzyme preparations can decompose a small amount of formaldehyde in the wood. After the curing reaction, an acetyl group protective layer is produced on the surface of the wood, which improves the flexibility of the wood fibers and increases the parallel extension force and bending tensile strength of the wood fibers.

[0061] Among them, the wood anti-corrosion paint in step six adopts Mugunghwa water-based wood anti-corrosion paint, which has high antibacterial activity, can inhibit the corrosion and damage of various bacteria, molds, fungi, etc. to wood fibers, and can form a protective paint film on the wood surface.

[0062] The use of Infinitus water-based wood anti-corrosion paint can make standard wood resist ultraviolet radiation, and be better waterproof, moisture-proof and mildew-proof. At the same time, it has super strong penetration and adhesion, can produce capillary action with wood, and form a lasting bond. It is harmless to the human body, can prevent fine dust, is dirt-resistant and easy to clean.

[0063] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0064] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing durable termite-proof wood, characterized in that: The specific steps are as follows: Step 1: Prepare good-quality wood materials, then use a cutting machine to split the wood materials into wood material segments of equal length, and then use a cutting device to cut the wood material segments, peel the wood material segments and cut them into wood of the same size; Step 2: Use drilling equipment to drill holes in the standard wood at certain intervals, then clean the drilled standard wood and remove sawdust and dust from the wood surface and holes; Step 2: Prepare anti-termite agent and silica sol, mix them in a ratio of 1:5, add them into a mixing tank and stir them thoroughly for 30 minutes to one hour, so that the anti-termite agent and silica sol are fully mixed to form a wood impregnation stock solution; Step 3: Put the treated standard wood into a pressure tank, then add the wood impregnation solution, and pressurize and impregnate for ten hours at 60 degrees Celsius and 1Mpa atmospheric pressure to make the wood impregnation solution fully penetrate into the standard wood. At this time, under the action of silica sol, the anti-termite agent will be firmly adsorbed on the inner layer of the standard wood. Then, vacuum pumping operation is performed to drain the excess solution in the pressure tank and take out the standard wood; Step 4: Put the impregnated standard wood into the drying box, then adjust the temperature to 80 degrees Celsius for drying. After 10 hours, take out the standard wood and cool it naturally to room temperature to dry out the excess moisture in the standard wood. Then test the moisture content inside the wood. If the moisture content is below 15%, you can continue the subsequent operation. If the moisture content is still over 15%, put the standard wood back into the drying box to continue the drying operation. Then use the fan to clean the dust attached to the outer surface of the cooled standard wood and the residual debris in the holes for a second time. After cleaning, prepare two parts of filler and one part of adhesive. , put them into a mixing barrel and stir and mix them in a ratio of 2:1 to make a wood filler, then put the wood filler into a vibration device for vibration treatment and take it out after thirty minutes, observe whether there are still bubbles inside the wood filler, if there are still bubbles, continue to use the vibration device to treat until the bubbles inside the wood filler are completely removed, and obtain a filling agent that meets the standards, and finally inject the prepared wood filler into the holes opened in the standard wood at room temperature, and then let it stand for 24 hours to allow the wood filler and the inner wall of the hole opened on the standard wood to fully adhere to each other, so as to fill the hole; Step 5: Use grinding equipment to carefully grind the filled standard wood to remove excess wood filler and bumps on the wood surface to make the surface of the standard wood smooth. After grinding, use vacuum equipment to clean up the debris and dust on the outer surface of the standard wood. Then, evenly apply a layer of wood enhancer on the surface of the standard wood to reinforce the standard wood to prevent the standard wood from cracking during subsequent use due to the opening of holes. Step 6: Pour the wood anticorrosive paint into a mixing bucket, stir evenly, add 0-20% clean water to dilute, and then stir thoroughly again to obtain the wood anticorrosive paint stock solution. Subsequently, a layer of the wood anticorrosive paint stock solution is evenly applied on the outer surface of the standard wood and placed in a well-ventilated place for natural ventilation. After 4 hours, a layer of the wood anticorrosive paint stock solution is applied again, and after ventilation and drying, the preparation of the durable termite-proof wood is completed.

2. The method for preparing a durable termite-proof wood according to claim 1, characterized in that: The certain intervals mentioned in step 2 can be drilled at intervals of 10 cm or 20 cm according to the size of the standard wood, and the depth of the holes can be selected to be fully penetrated or half-penetrated according to the thickness of the standard wood.

3. The method for preparing a durable termite-proof wood according to claim 1, characterized in that: The anti-termite agent described in step 3 is made of 5% concentration of sulfluramid reagent, which is an organic fluorine termiticide.

4. The method for preparing a durable termite-proof wood according to claim 1, characterized in that: The silica sol described in step 3 will be dehydrated to generate silicon dioxide after being heated. Silicon dioxide has a high specific surface area and can effectively absorb the anti-termite agent and fill the interior of the wood.

5. The method for preparing a durable termite-proof wood according to claim 1, characterized in that: During the drying process of the dimensional wood described in step 4, it is necessary to ensure that the dimensional wood maintains a constant weight after drying.

6. The method for preparing a durable termite-proof wood according to claim 1, characterized in that: The filler described in step 4 is made of calcium stearate, which is a naturally curable inorganic filler that can fill cracks and holes on the surface of wood.

7. The method for preparing a durable termite-proof wood according to claim 1, characterized in that: The adhesive described in step 4 is made of polyurethane, which is a commonly used adhesive and has good filling and bonding properties when filling cracks and holes on the surface of wood.

8. The method for preparing a durable termite-proof wood according to claim 1, characterized in that: The wood enhancer described in step five mainly includes modified polyurethane and active enzyme preparations, which are used to improve the hardness, strength, weather resistance, corrosion resistance, moisture resistance and waterproofness of standard wood, and to seal the unpleasant odors such as grease inside the wood, and the infiltration and volatilization of chemical substances such as formaldehyde.

9. The method for preparing a durable termite-proof wood according to claim 1, characterized in that: The wood anticorrosive paint described in step six uses Mugunghwa water-based wood anticorrosive paint, which has high antibacterial activity, can inhibit the corrosion and damage of various bacteria, molds, fungi, etc. to wood fibers, and can form a protective paint film on the wood surface.