Moisture-heat-resistant fiber-reinforced resin-based composite material and preparation method thereof

By using silicone-modified epoxy resin and specific process parameters, the performance of carbon fiber reinforced resin matrix composites in humid and hot environments has been improved, solving the problem of performance degradation under humid and hot conditions and realizing composite materials with high strength and low porosity.

CN118906571APending Publication Date: 2024-11-08ZHONGFU SHENYING CARBON FIBER
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410978462.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Traditional carbon fiber reinforced resin matrix composites are prone to moisture absorption in humid and hot environments, which leads to performance degradation and affects their reliability and durability in complex service environments.

Method used

Using silicone-modified epoxy resin as an adhesive, and by controlling the ratio of the fiber areal density of the unidirectional prepreg tape to the areal density of the equalizing plate, combined with specific curing process parameters, a three-dimensional network structure is formed, which improves the interfacial bonding force between the resin and the fiber and the resistance to damp heat.

Benefits of technology

The composite material achieved high interlayer shear strength and strength retention rate under humid and hot conditions, reduced porosity, and improved interfacial properties and resistance to humid and hot conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118906571A_ABST
    Figure CN118906571A_ABST
Patent Text Reader

Abstract

The invention discloses a damp-heat-resistant fiber-reinforced resin-based composite material, and relates to the technical field of composite materials. The composite material comprises one-way infiltrating belts which are arranged in a stacked mode, and the fiber surface density of the one-way infiltrating belts is 180-210 g / m < 2 >. The interlaminar shear strength of the composite material can reach 95 MPa, the damp-heat interlaminar shear strength reaches 66 MPa, the strength damp-heat retention rate reaches 70%, the porosity can be 0.16%, and the composite material has excellent interface performance and damp-heat resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of composite materials, and in particular to a moisture and heat resistant fiber reinforced resin-based composite material and a preparation method thereof. Background Art

[0002] Composite materials used in aircraft structures must not only withstand complex, long-term fatigue loads, accidental impact loads, etc., but also withstand the test of harsh external environmental factors such as temperature and humidity. With the continuous improvement of aircraft performance, the performance requirements for structural composite materials are also getting higher and higher. At the same time, composite materials themselves have component diversity, structural multiplicity, and failure mode diversity. These characteristics make the performance evolution analysis of composite materials very complicated. For resin-based structural composite materials, the influence of humid and hot environmental conditions on the mechanical properties of composite materials is very obvious, which can lead to a decrease in the strength and stiffness of composite materials.

[0003] The advantages of carbon fiber reinforced resin-based composites (CFRP) such as high specific strength modulus, high temperature resistance, corrosion resistance, fatigue resistance, good damage safety, and performance designability have been recognized by the world, and have gradually become the preferred material for advanced national defense equipment. However, it is well known that the traditional resin matrix has a certain polarity and is easy to absorb moisture in a hot and humid environment. The plasticization and swelling effect of the absorbed moisture on the matrix and the micro cracks caused by the internal stress generated by the mismatch between the wet and thermal expansion coefficients of the resin and the fiber cause a sharp decline in the performance of the composite material. The existence of these problems will seriously affect the reliable application of domestic carbon fiber composites. Therefore, the wet and hot performance of domestic carbon fiber composites in service environments can be used as a key characteristic to measure their durability and damage tolerance. Its research is an important guarantee and prerequisite for promoting its application. Summary of the invention

[0004] In order to solve the above technical problems, the present application aims to provide a moisture and heat resistant carbon fiber reinforced resin-based composite material and a preparation method thereof, wherein the composite material has excellent interface properties and moisture and heat resistance.

[0005] According to the first aspect of the present application, a moisture-heat resistant fiber-reinforced resin-based composite material comprises a stacked unidirectional impregnation tape, wherein the fiber surface density of the unidirectional impregnation tape is 180-210 g / m 2 .

[0006] In some embodiments of the present application, the composite material further includes an adhesive for curing the stacked unidirectional impregnation tapes, and the mass of the adhesive accounts for 30-40% of the total mass of the composite material.

[0007] In some embodiments of the present application, the adhesive is formed by curing a dipping solution, wherein the dipping solution includes an organic solvent and a silicone-modified epoxy resin in a weight ratio of 10:6-8.

[0008] According to a second aspect of the present application, a method for preparing a composite material is provided. The method for preparing a composite material is used to prepare the above-mentioned moisture-heat-resistant fiber-reinforced resin-based composite material. The method comprises:

[0009] Laying and stacking multiple layers of the unidirectional prepreg tapes to form a preform;

[0010] Laying a pressure equalizing plate on the prefabricated part to form a preformed structure;

[0011] The preformed structure is cured under preset conditions to obtain the composite material.

[0012] In some embodiments of the present application, the preparation method further comprises:

[0013] Passing the continuous fiber bundle through the dipping solution to form a dipping fiber bundle;

[0014] The impregnated fiber bundles are arranged in parallel at preset intervals and dried to form the unidirectional prepreg tape.

[0015] In some embodiments of the present application, the density of the pressure balancing plate is 7.5-8.5 g / cm 3 , thickness is 4.5-5.5mm.

[0016] In some embodiments of the present application, the ratio of the surface density of the pressure equalizing plate to the fiber surface density of the prepreg tape is 182.1-222.6.

[0017] In some embodiments of the present application, the surface roughness of the pressure equalizing plate is 0.4-0.8 μm.

[0018] In some embodiments of the present application, the preset conditions include:

[0019] Under the preset vacuum degree, pressurize to 0.6-1.0MPa at the preset pressurization rate, heat to 60-80℃ at the preset heating rate, and keep the temperature and pressure for 60-80min; continue to heat to 120-140℃ at the preset heating rate, and keep the temperature and pressure for 130-200min.

[0020] In some embodiments of the present application, the preset heating rate is 1 to 5°C / min, the preset pressurization rate is 0.01 to 0.05 MPa / min, and the preset vacuum degree is -0.090 to -0.098 MPa.

[0021] The technical solution provided by this application may have the following beneficial effects:

[0022] The composite material of the present application has an interlaminar shear strength of 95 MPa, a wet heat interlaminar shear strength of 66 MPa, a wet heat retention rate of strength of 70%, a porosity of 0.16%, and has excellent interface performance and wet heat resistance.

[0023] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0025] Figure 1 The present invention is a flow chart of a method for preparing a composite material according to an exemplary embodiment.

[0026] Figure 2 FIG. 4 is a schematic diagram of a layer structure of a preformed structure according to an exemplary embodiment.

[0027] Figure 3 The present invention is a flow chart showing a method for preparing a unidirectional prepreg tape according to an exemplary embodiment.

[0028] Figure 4 This is a metallographic microscope image of the laminate of Example 1.

[0029] Figure 5 This is a magnified metallographic microscope image of the laminate of Example 1. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme of the present application will be clearly and completely described below in combination with the embodiments of the present application and the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present application. It should be noted that, in the absence of conflict, the embodiments in the present application and the features in the embodiments can be arbitrarily combined with each other.

[0031] The present application provides a moisture-heat resistant fiber-reinforced resin-based composite material, which includes a stacked unidirectional prepreg tape, the fiber surface density of the prepreg tape is 180-210g / m 2 The interlaminar shear strength of the composite material of the present application can reach 95MPa, the wet heat interlaminar shear strength can reach 66MPa, the wet heat retention rate of strength can reach 70%, the porosity can be 0.16%, and it has excellent interface performance and wet heat resistance.

[0032] An exemplary embodiment of the present application provides a moisture-heat resistant fiber-reinforced resin-based composite material, the composite material includes stacked unidirectional impregnation tapes, the fiber surface density of the unidirectional impregnation tapes is 180-210 g / m 2 .

[0033] In this embodiment, the fiber surface density of the unidirectional prepreg tape is controlled to be 180-210 g / m 2 , which is beneficial to improve the mechanical properties of the composite material. The interlaminar shear strength of the composite material obtained can reach 95MPa, the wet heat interlaminar shear strength can reach 66MPa, the wet heat retention rate of the strength can reach 70%, and the porosity can be 0.16%, which has excellent interface performance and wet heat resistance. For example, the fiber surface density of the unidirectional prepreg tape is 180g / m 2 , 189g / m 2 , 194g / m 2 , 199g / m 2 , 205g / m 2 or 210g / m 2 .

[0034] In an exemplary embodiment, the composite material further comprises an adhesive for curing the stacked unidirectional impregnation tapes, and the mass of the adhesive accounts for 30-40% of the total mass of the composite material.

[0035] In this embodiment, a three-dimensional network structure can be formed by curing the adhesive to provide a stable geometric shape and dimensional stability for the composite material. In addition, the adhesive provides shear force transmission between the layers of the composite material to enhance interlayer bonding and improve the overall performance of the composite material. The mass of the adhesive is controlled at 30-40% of the total mass of the composite material, which can balance the tensile strength, impact toughness, interlayer shear strength, moisture and heat resistance, and bonding properties of the composite material. Exemplarily, the mass of the adhesive accounts for 30%, 34%, 37% or 40% of the total mass of the unidirectional prepreg.

[0036] In an exemplary embodiment, the adhesive is formed by curing a dipping solution, wherein the dipping solution includes an organic solvent and an organosilicon-modified epoxy resin in a weight ratio of 10:6-8.

[0037] Because epoxy resin has the advantages of high mechanical strength, good chemical stability, high bonding strength and low shrinkage, it is a thermosetting resin material commonly used in composite materials, but because the water absorption of common epoxy resin is high, the resistance to moisture and heat is poor, which limits the application of composite materials prepared by it under moist and hot environments. Therefore, the present embodiment uses organosilicon-modified epoxy resin as the main resin material, and because the organosilicon-modified epoxy resin introduces flexible silicon oxygen segments, its surface hydrophobicity is improved, which can not only improve the water resistance and chemical medium erosion resistance of the modified epoxy resin, but also improve the toughness and thermal stability of the modified epoxy resin. In the present embodiment, the organosilicon-modified epoxy resin is solid, therefore, in order to facilitate its impregnation of continuous fiber bundles, the organosilicon-modified epoxy resin can be crushed, mixed with an organic solvent, to form a dipping solution. Wherein, the organosilicon-modified epoxy resin can be selected from Beston Composite Materials (Wuhan) Co., Ltd.

[0038] For example, the weight ratio of the organic solvent to the organosilicon-modified epoxy resin may be 10:6, 10:6.5, 10:7 or 10:8. To facilitate the curing of the dipping solution to form a glue, the organic solvent may be a low-boiling point organic solvent, for example, the organic solvent may be acetone.

[0039] like Figure 1 As shown, an exemplary embodiment of the present application provides a method for preparing a composite material, and the preparation method includes:

[0040] S110, stacking multiple layers of unidirectional prepreg tapes to form a preform.

[0041] Before step S110, the mold may be cleaned with a soft material, and then a mold release agent may be applied to the mold; and then multiple layers of unidirectional prepreg tapes may be stacked to form a preform. The stacking angles and the number of layers of the unidirectional prepreg tapes are not limited. For example, a [45 / -45]S or [0 / 90]S laying method may be used; and the number of layers may be 6-20.

[0042] S120, laying a pressure equalizing plate on the prefabricated part to form a preformed structure.

[0043] In step S120, by laying a pressure plate on the preform, the surface flatness of the composite material can be improved on the one hand, and the porosity of the composite material can be reduced on the other hand by the pressing effect of the pressure plate on the preform. The pressure plate can be a metal plate with a smooth surface. For example, the pressure plate can be a 45 alloy steel plate.

[0044] In this embodiment, the composite material can be prepared by using an autoclave molding process, the preform, the pressure equalizing plate and other auxiliary materials are combined and placed in a vacuum bag, and then the vacuum bag is sealed with a sealing strip.

[0045] Among them, the preformed structure is as follows Figure 2 As shown, Figure 2 In the figure, from bottom to top, there are mold 1, first non-porous isolation film layer 21, first demoulding cloth layer 31, preform layer 4, first demoulding cloth layer 32, second non-porous isolation film layer 22, adhesive absorbing material layer 5, equalizing plate layer 6, breathable material layer 7, vacuum bag 8, wherein a sealing strip layer 9 is provided between the vacuum bag 8 and the mold 1. The main function of the first demoulding cloth layer 31 and the second demoulding cloth layer 32 is to facilitate the smooth demoulding of the cured composite material from the mold 1. The materials of the first demoulding cloth layer 31 and the second demoulding cloth layer 32 can be the same, for example, both are made of polyethylene terephthalate (PET), polyamide (PA), etc. The main function of the first non-porous isolation film layer 21 and the second non-porous isolation film layer 22 is to facilitate the smooth demoulding of the cured composite material from the mold 1, and at the same time, it can also protect the surface of the composite material to reduce wear; the material of the first non-porous isolation film layer 21 and the second non-porous isolation film layer 22 can be the same, for example, polyethylene (PE), polypropylene (PP), polytetrafluoroethylene (PTFE), etc. The glue absorbing material layer 5 is used to absorb excess dipping liquid during the flow and curing process of the dipping liquid, for example, polyester, polyamide and other materials can be used. The main function of the breathable material layer 7 is to allow air and volatile gases to escape from the preform layer 4 during the curing process, while preventing the dipping liquid from flowing out of the vacuum bag 8, for example, PET, PA and other materials can be used.

[0046] S130, curing the preformed structure under preset conditions to obtain a composite material.

[0047] In this embodiment, after the continuous fiber bundle passes through the impregnation liquid, an impregnated fiber bundle is formed; the impregnated fiber bundle is arranged in parallel at a preset interval, and after drying, part of the organic solvent therein can be removed to form a unidirectional prepreg tape; after multiple layers of unidirectional prepreg tapes are laid and stacked, a preformed part is formed; a pressure equalizing plate is laid on the preform to form a preformed structure, and when the preformed structure is cured under preset conditions, the resin in the impregnation liquid is cured to form a three-dimensional network structure of adhesive to improve the bonding strength between the layers.

[0048] In an exemplary embodiment, before step S110 in the above embodiment, as Figure 3 As shown, the method for preparing the composite material also includes:

[0049] S210, passing the continuous fiber bundle through the impregnation liquid to form an impregnated fiber bundle.

[0050] In step S210, the continuous fiber bundle is passed through the dipping solution, and one or more guide rollers are used to remove excess dipping solution on the surface of the continuous fiber bundle to form a dipping fiber bundle. The continuous fiber bundle can be, for example, dry-jet wet-spun T700 grade (SYT49C-12K) carbon fiber.

[0051] S220, arranging the impregnated fiber bundles in parallel at a preset interval, and forming a unidirectional prepreg tape after drying.

[0052] In step S220, a unidirectional prepreg tape can be prepared by a drum winding method. For example, a layer of release paper is laid flat on the drum of the winding device, and the impregnated fiber bundles are wound around the drum in parallel. When the drum rotates, the impregnated fiber bundles are wound around the drum in parallel at a preset interval, and then the wound impregnated fiber bundles are cut and unfolded along a main line of the drum, and the organic solvent on the surface of the impregnated fiber bundles is dried and removed to obtain a unidirectional prepreg tape. The preset interval can be determined according to the impregnation process and product performance requirements; for example, by adjusting the motor frequency of the winding device to adjust the rotation speed of the drum and the preset interval, the fiber surface density of the unidirectional prepreg tape can be controlled at 180-210g / m 2 .

[0053] In an exemplary embodiment, the density of the pressure plate is 7.5-8.5 g / cm 3 , thickness is 4.5-5.5mm.

[0054] In this embodiment, the density of the pressure balancing plate can be 7.5 g / cm 3 , 8.0g / cm 3 or 8.5g / cm 3 ; The thickness can be 4.5mm, 5.0mm or 5.5mm.

[0055] In an exemplary embodiment, the ratio of the area density of the press plate to the fiber area density of the prepreg tape is 182.1-222.6.

[0056] In this embodiment, by controlling the ratio of the surface density of the pressure plate to the fiber surface density of the prepreg tape within 182.1-222.6, the composite material can have good mechanical properties and moisture and heat resistance. For example, the ratio of the surface density of the pressure plate to the fiber surface density of the prepreg tape is 182.1, 193.7, 209.2, 215.6 or 222.6.

[0057] In an exemplary embodiment, the surface roughness of the pressure equalizing plate is 0.4-0.8 μm.

[0058] Surface roughness refers to the measurement of the tiny unevenness on the surface of an object, which is used to describe the smoothness of the material surface. The level of surface roughness is usually divided according to the Ra value, which can range from 0.025μm to 100μm. In this embodiment, the surface roughness of the equalizing plate is 0.4-0.8μm. Placing the equalizing plate on the preform can improve the surface flatness of the preform. Exemplarily, the surface roughness of the equalizing plate is 0.4μm or 0.8μm.

[0059] In an exemplary embodiment, the preset conditions include:

[0060] Under the preset vacuum degree, pressurize to 0.6-1.0MPa at the preset pressurization rate, heat to 60-80℃ at the preset heating rate, and keep the temperature and pressure for 60-80min; continue to heat to 120-140℃ at the preset heating rate, and keep the temperature and pressure for 130-200min.

[0061] In this embodiment, curing is performed by heating at 60-80°C / 60-80min+120-140°C / 130-200min in two stages, and the curing pressure is controlled at 0.6-1.0MPa, which can effectively enhance the crosslinking degree of the epoxy resin, improve the interface bonding strength between the epoxy resin and the fiber, and reduce the porosity of the composite material. After the preformed structure is cured by the above curing system, the temperature can be kept at 2.0°C / min to below 60°C, and the pressure can be released out of the tank.

[0062] Exemplarily, in one embodiment, the preset conditions include:

[0063] Under the preset vacuum degree, the pressure is increased to 0.6MPa at the preset pressure rate, the temperature is increased to 60°C at the preset heating rate, and the temperature is kept at this temperature for 80 minutes; the temperature is continued to be increased to 120°C at the preset heating rate, and the temperature is kept at this temperature for 200 minutes.

[0064] In another embodiment, the preset conditions include:

[0065] Under the preset vacuum degree, the pressure is increased to 0.8 MPa at the preset pressure rate, the temperature is increased to 70°C at the preset heating rate, and the temperature is kept at this temperature for 70 minutes; the temperature is continued to be increased to 130°C at the preset heating rate, and the temperature is kept at this temperature for 160 minutes.

[0066] In another embodiment, the preset conditions include:

[0067] Under the preset vacuum degree, the pressure is increased to 1.0 MPa at the preset pressure rate, the temperature is increased to 80°C at the preset heating rate, and the temperature is kept at this temperature for 60 minutes; the temperature is continued to be increased to 140°C at the preset heating rate, and the temperature is kept at this temperature for 130 minutes.

[0068] In an exemplary embodiment, the preset heating rate is 1 to 5° C. / min, the preset pressurization rate is 0.01 to 0.05 MPa / min, and the preset vacuum degree is -0.090 to -0.098 MPa.

[0069] In this embodiment, by controlling the preset heating rate at 1-5°C / min and the preset pressurization rate at 0.01-0.05MPa / min, it is beneficial to maintain the stability of the curing process and avoid stress differences and deformation problems caused by excessive differences in internal and external stresses of the composite material due to rapid changes in temperature or pressure.

[0070] Exemplarily, in one embodiment, the preset heating rate is 1° C. / min, the preset pressurization rate is 0.01 MPa / min, and the preset vacuum degree is -0.090 MPa.

[0071] In another embodiment, the preset heating rate is 3° C. / min, the preset pressurization rate is 0.03 MPa / min, and the preset vacuum degree is -0.094 MPa.

[0072] In another embodiment, the preset heating rate is 5° C. / min, the preset pressurization rate is 0.05 MPa / min, and the preset vacuum degree is -0.098 MPa.

[0073] In order to more clearly explain the technical solution of the present application, the present application lists specific examples of the method for preparing the composite material, and the beneficial effects of selecting the above ranges of each process parameter will be explained by giving specific experimental data through specific examples.

[0074] Example

[0075] Embodiment 1: A method for preparing a composite material, comprising the following steps:

[0076] (1) The organosilicon-modified epoxy resin is crushed, mixed with acetone in a weight ratio of 10:6.5, and stirred until the organosilicon-modified epoxy resin is dissolved to obtain a dipping solution.

[0077] (2) The continuous carbon fiber bundle is passed through a dipping solution to form a dipping fiber bundle.

[0078] (3) The fiber bundles after impregnation are arranged in parallel at a preset interval by the drum winding method. After drying, the fiber surface density is 194 g / m 2 Unidirectional prepreg tape.

[0079] (4) Composite laminates are prepared by an autoclave method, and multiple layers of unidirectional prepreg tapes are stacked to form a preform.

[0080] (5) Combine the preform with the pressure plate and other auxiliary materials and put them into a vacuum bag, and seal the vacuum bag with a sealing strip to form a preformed structure. The pressure plate is made of 45# alloy steel with a density of 7.85g / cm 3 , thickness is 5.0 mm, surface roughness is 0.8; the ratio of the surface density of the equalizing plate to the fiber surface density of the prepreg tape is 202.3.

[0081] (6) The preformed structure is cured under the preset conditions, and the preset conditions (curing process parameters) are: evacuate at room temperature (25°C) to make the vacuum degree in the vacuum bag -0.095MPa; start pressurizing at room temperature and pressurize to 1.0MPa at a rate of 0.02MPa / min; then heat to 70°C at a rate of 1.5°C / min, and keep the temperature and pressure for 70min; continue to heat to 130°C at a rate of 1.5°C / min, and keep the temperature and pressure for 175min; then cool to below 60°C at a rate of 2.0°C / min, and release the pressure out of the tank; the preformed structure's impregnation liquid is cured to form a cured preform adhesive to obtain a composite material (laminated plate). Among them, the mass of the adhesive in the composite material accounts for 34% of the total mass of the composite laminate.

[0082] The metallographic microscope image of the composite laminate in this embodiment is as follows: Figure 4 and Figure 5 As shown, from Figure 4 It can be seen that the layers are evenly arranged without obvious cracks or gaps, indicating that the laminate has good mechanical properties and durability. Figure 5 It can be seen that there are fewer black dot-like structures in the laminate, indicating that the laminate has a lower porosity.

[0083] Embodiment 2: A method for preparing a composite material, comprising the following steps:

[0084] (1) The organosilicon-modified epoxy resin is crushed, mixed with acetone in a weight ratio of 10:6, and stirred until the organosilicon-modified epoxy resin is dissolved to obtain a dipping solution.

[0085] (2) The continuous carbon fiber bundle is passed through a dipping solution to form a dipping fiber bundle.

[0086] (3) The fiber bundles after impregnation are arranged in parallel at a preset interval by the drum winding method. After drying, the fiber surface density is 194 g / m 2 Unidirectional prepreg tape.

[0087] (4) Composite laminates are prepared by an autoclave method, and multiple layers of unidirectional prepreg tapes are stacked to form a preform.

[0088] (5) Combine the preform with the pressure plate and other auxiliary materials and put them into a vacuum bag, and seal the vacuum bag with a sealing strip to form a preformed structure. The pressure plate is made of 45# alloy steel with a density of 7.85g / cm 3 , thickness is 4.5mm, surface roughness is 0.4; the ratio of the surface density of the equalizing plate to the fiber surface density of the prepreg tape is 182.1.

[0089] (6) The preformed structure is cured under the preset conditions, and the preset conditions (curing process parameters) are: evacuate at room temperature (25°C) to make the vacuum degree in the vacuum bag -0.090MPa; start pressurizing at room temperature and pressurize to 0.6MPa at a rate of 0.01MPa / min; then heat to 60°C at a rate of 1°C / min, and keep the temperature and pressure for 80 minutes; continue to heat to 120°C at a rate of 1°C / min, and keep the temperature and pressure for 200 minutes; then cool to below 60°C at a rate of 2.0°C / min, keep the pressure, and release the pressure out of the tank; the impregnation liquid of the preformed structure is cured to form a glue for curing the preform, and obtain a composite material (laminated plate). Among them, the mass of the glue in the composite material accounts for 30% of the total mass of the composite laminate.

[0090] Embodiment 3: A method for preparing a composite material, comprising the following steps:

[0091] (1) The organosilicon-modified epoxy resin is crushed, mixed with acetone in a weight ratio of 10:8, and stirred until the organosilicon-modified epoxy resin is dissolved to obtain a dipping solution.

[0092] (2) The continuous carbon fiber bundle is passed through a dipping solution to form a dipping fiber bundle.

[0093] (3) The fiber bundles after impregnation are arranged in parallel at a preset interval by the drum winding method. After drying, the fiber surface density is 194 g / m 2 Unidirectional prepreg tape.

[0094] (4) Composite laminates are prepared by an autoclave method, and multiple layers of unidirectional prepreg tapes are stacked to form a preform.

[0095] (5) Combine the preform with the pressure plate and other auxiliary materials and put them into a vacuum bag, and seal the vacuum bag with a sealing strip to form a preformed structure. The pressure plate is made of 45# alloy steel with a density of 7.85g / cm 3 , thickness is 5.5mm, surface roughness is 0.8; the ratio of the surface density of the equalizing plate to the fiber surface density of the prepreg tape is 222.6.

[0096] (6) The preformed structure is cured under the preset conditions, and the preset conditions (curing process parameters) are: evacuate at room temperature (25°C) to make the vacuum degree in the vacuum bag -0.098MPa; pressurize at room temperature and pressurize at a rate of 0.05MPa / min to 1.0MPa; then heat to 80°C at a rate of 5°C / min, and keep the temperature and pressure for 60min; continue to heat to 140°C at a rate of 5°C / min, and keep the temperature and pressure for 130min; then cool to below 60°C at a rate of 2.0°C / min, keep the pressure, and release the pressure out of the tank; the impregnation liquid of the preformed structure is cured to form a glue for curing the preform, and obtain a composite material (laminated plate). Among them, the mass of the glue in the composite material accounts for 40% of the total mass of the composite laminate.

[0097] In order to more clearly explain the technical solution of the present application, the present application also lists Examples 4-12 of the preparation method of the composite material, wherein the process parameters of Examples 4-12 are shown in Table 1.

[0098] Table 1 Process parameters of composite materials

[0099]

[0100] Table 1 (Continued) Process parameters of composite materials

[0101]

[0102] Performance Testing

[0103] The properties of the laminate prepared in the example were tested according to the following method, and the test results are recorded in Table 2.

[0104] 1. Interlaminar shear strength: The interlaminar shear strength of the laminate was tested according to the method in ASTM D2344, where the interlaminar shear strength includes the interlaminar shear strength (ILSS) under conventional test conditions (23°C / 50% RH) and the interlaminar shear strength under wet heat conditions (boiled in deionized water at 100°C for 3 days) (ILSS-ETW).

[0105] 2. Porosity: The laminate is observed using a metallographic microscope and the number of pores per unit area is measured to calculate the porosity of the composite material.

[0106] Table 2 Performance test table of the laminated board of the embodiment

[0107] ILSS, MPa ILSS-ETW, MPa Strength moisture retention rate, % Porosity, % Example 1 95.0 66.7 70.2 0.16 Example 2 90.5 61.6 68.1 0.19 Example 3 92.8 64.0 69.0 0.16 Example 4 85.3 59.1 69.3 0.17 Example 5 90.6 64.0 70.6 0.18 Example 6 93.1 64.7 69.5 0.17 Example 7 94.5 65.0 68.8 0.19 Example 8 94.0 64.2 68.3 0.19 Example 9 91.3 62.1 68.0 0.21 Example 10 87.4 59.8 68.4 0.25 Embodiment 11 85.6 54.3 63.4 0.34 Example 12 82.5 47.5 57.6 0.48

[0108] Combining the data in Table 1 and Table 2, it can be seen that the interlaminar shear strength, wet heat interlaminar shear strength, and wet heat retention rate of the laminate of Example 1 are significantly better than those of the laminates of Examples 9-12, indicating that when preparing composite laminates, using an equalizing plate to prepare a preformed structure can improve the interfacial bonding force between the resin and the fiber; at the same time, the wet heat retention rate of the laminate of Example 1 is significantly higher than that of the laminates of Examples 9-12, and the porosity of the laminate of Example 1 is significantly lower than that of the laminates of Examples 9-12, indicating that under wet heat conditions, the water absorption capacity of the interface between the resin and the fiber decreases, the plasticization and swelling effects weaken, and the movement of the resin molecular chain slows down, so that the mechanical properties of the composite material are maintained.

[0109] The interlaminar shear strength, wet heat interlaminar shear strength, and wet heat retention rate of the laminate of Example 1 are significantly better than those of the laminates of Examples 2-4, indicating that when preparing composite laminates, by adjusting the curing process parameters, the cross-linking degree of the epoxy resin can be effectively enhanced, thereby improving the interfacial bonding strength between the resin and the fiber; at the same time, it is beneficial to reduce the porosity of the composite material, indicating that the interface performance and wet heat resistance of the composite material can be improved by adjusting the curing process parameters.

[0110] The interlaminar shear strength, wet heat interlaminar shear strength, and wet heat retention rate of the laminate of Example 1 are significantly better than those of the laminates of Examples 5-8, indicating that when preparing composite laminates, the interface properties and wet heat resistance of the composite material can be improved by adjusting the fiber surface density of the prepreg tape and the ratio of the surface density of the equalizing plate to the prepreg tape.

[0111] In summary, the composite material of the present application has an interlaminar shear strength of 95 MPa, a wet heat interlaminar shear strength of 66 MPa, a wet heat retention rate of strength of 70%, a porosity of 0.16%, and has excellent interface properties and wet heat resistance.

[0112] It should be noted that, in this article, the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0113] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application is described in detail with reference to the above embodiments, a person skilled in the art should understand that the technical solutions described in the above embodiments can still be modified, or some of the technical features can be replaced by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present application.

Claims

1. A moisture and heat resistant fiber reinforced resin-based composite material, characterized in that: The composite material comprises stacked unidirectional impregnation tapes, wherein the fiber surface density of the unidirectional impregnation tapes is 180-210 g / m 2 .

2. The moisture-heat resistant fiber-reinforced resin-based composite material according to claim 1, characterized in that: The composite material further comprises an adhesive for curing the stacked unidirectional impregnation tapes, and the mass of the adhesive accounts for 30-40% of the total mass of the composite material.

3. The moisture-heat resistant fiber-reinforced resin-based composite material according to claim 2, characterized in that: The adhesive is formed by curing a dipping solution, wherein the dipping solution comprises an organic solvent and an organosilicon-modified epoxy resin in a weight ratio of 10:6-8.

4. A method for preparing a composite material, characterized in that: The preparation method of the composite material is used to prepare the moisture-heat resistant fiber-reinforced resin-based composite material according to any one of claims 1 to 3, and the preparation method comprises: Laying and stacking multiple layers of the unidirectional prepreg tapes to form a preform; Laying a pressure equalizing plate on the prefabricated part to form a preformed structure; The preformed structure is cured under preset conditions to obtain the composite material.

5. The method for preparing a composite material according to claim 4, characterized in that: The preparation method further comprises: Passing the continuous fiber bundle through the dipping solution to form a dipping fiber bundle; The impregnated fiber bundles are arranged in parallel at preset intervals and dried to form the unidirectional prepreg tape.

6. The method for preparing a composite material according to claim 4, characterized in that: The density of the pressure balancing plate is 7.5-8.5 g / cm 3 , thickness is 4.5-5.5mm.

7. The method for preparing a composite material according to claim 4, characterized in that: The ratio of the surface density of the pressure balancing plate to the fiber surface density of the prepreg tape is 182.1-222.

6.

8. The method for preparing a composite material according to claim 4, characterized in that: The surface roughness of the pressure balancing plate is 0.4-0.8 μm.

9. The method for preparing a composite material according to claim 4, characterized in that: The preset conditions include: Under the preset vacuum degree, pressurize to 0.6-1.0MPa at the preset pressurization rate, heat to 60-80℃ at the preset heating rate, and keep the temperature and pressure for 60-80min; continue to heat to 120-140℃ at the preset heating rate, and keep the temperature and pressure for 130-200min.

10. The method for preparing a composite material according to claim 9, characterized in that: The preset heating rate is 1 to 5°C / min, the preset pressurization rate is 0.01 to 0.05MPa / min, and the preset vacuum degree is -0.090 to -0.098MPa.

Citation Information

Patent Citations

  • Impact-resistant lightweight density gradient composite material, fan containment casing, preparation method and application thereof

    CN109278372A

  • Method for testing pressure-thickness ratio of prepreg of resin-based composite material

    CN117325481A

  • Sizing agent and preparation method thereof, carbon fiber and composite material

    CN118029157A