Method for preparing NFPP material as sodium ion battery positive electrode material by double organic molecule template method

The dual organic molecular template method optimizes its microstructure in the sodium ion battery positive electrode material NFPP, which solves the problem of insufficient electronic conductivity and ion diffusion of NFPP materials, significantly improves its electrochemical performance, and is suitable for industrial production.

CN118908171AInactive Publication Date: 2024-11-08LEPU SODIUM ELECTRIC NEW MATERIALS (LUAN) CO LTD

Patent Information

Application Number
CN202410956803.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing sodium ion battery positive electrode material NFPP has a low electronic conductivity and poor ion diffusion, which leads to its limited electrochemical performance, which restricts its practical application.

Method used

The NFPP material was prepared by the dual organic molecular template method, and the gel-like precursor was formed by adding alkali metal sources, iron sources, phosphate root sources and doping elements to the aqueous solution, and using complexing agents such as citric acid and glycine for two steps to form a gel-like precursor. , and then two-stage calcination was performed under an inert atmosphere to form a uniform carbon cladding layer, optimizing the microstructure of the NFPP composite.

Benefits of technology

It improves the electronic conductivity and ion diffusion rate of NFPP materials, significantly improves its electrochemical performance, including high reversible capacity, good cycling stability and excellent rate performance, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908171A_ABST
    Figure CN118908171A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing an NFPP material as a sodium ion battery positive electrode material by a double organic molecule template method, and the preparation method comprises the following steps: (1) sequentially adding an alkali metal source, an iron source, a phosphate radical source, different doping ions and two different complexing agents into a solvent, and heating and stirring to obtain a uniformly mixed precursor; (2) transferring the precursor obtained in the step (1) into a vacuum oven, and further baking; (3) calcining the sample obtained in the step (2) in a tubular furnace in an inert gas atmosphere, and cooling along with the furnace; and (4) sieving the cooled sintered material in the step (3) to obtain the modified polyanion mixed phosphoric acid system positive electrode material prepared by the double complexing agents. The preparation method of double organic molecule template induction is put into the production of the carbon-coated polyanionic positive electrode material for the first time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polyanion positive electrode materials for sodium ion batteries, and specifically relates to a method for preparing NFPP materials by a dual organic molecular template method for use as positive electrode materials for sodium ion batteries. Background Art

[0002] Sodium-ion batteries (SIBs) have attracted much attention due to their abundant resources, low cost and environmental friendliness, and are seen as a promising energy storage system to supplement and replace lithium-ion batteries. Compared with lithium-ion batteries, the sodium element used in sodium-ion batteries has large reserves, wide distribution and low price, which reduces dependence on a few metal resources and is more environmentally friendly and sustainable. However, compared with lithium-ion batteries, the development of sodium-ion batteries is still at a relatively backward stage and there is still a certain gap from achieving commercial application. Among them, the development of high-performance, low-cost cathode materials is one of the key bottlenecks in the development of sodium-ion batteries.

[0003] The cathode materials of sodium ion batteries mainly include transition metal oxides, Prussian blue analogs and polyacid salt compounds. Transition metal oxides such as NaFeO2, Na 2 / 3 Ni 1 / 3 Mn 2 / 3 Although O2 has a high theoretical specific capacity, it is easy to decompose in the air and has an unstable structure. In addition, the embedding / de-embedding process of transition metal ions will produce large volume deformation and irreversible structural changes, resulting in poor cycle stability and safety.

[0004] Prussian blue analogs such as sodium iron cobaltate have open skeleton structures and fast ion diffusion channels, high theoretical capacity and moderate average operating voltage. However, due to many defects, poor thermal stability, large volume expansion and other problems, their practical application prospects are greatly limited.

[0005] In contrast, polyacid salt compounds have attracted widespread attention due to their stable structure, small volume deformation and fast ion diffusion rate. Na3V2(PO4)3, Na3V2(PO4)2F3, NaVPO4F, etc. have been developed and used as positive electrode materials for sodium ion batteries. Among them, Na4Fe3(PO4)2P2O7(NFPP) is regarded as a low-cost, environmentally friendly positive electrode material with great application prospects due to its high theoretical specific capacity (129mAh / g), moderate average operating voltage (>3.1V) and small volume expansion (<4%).

[0006] However, the intrinsic electronic conductivity of NFPP is low and the ion diffusion is relatively slow, which seriously restricts its electrochemical performance. To solve this problem, researchers have used various strategies to improve the electronic conductivity and ion diffusivity of NFPP, such as nano-sizing, composite conductive additives, and construction of hollow / porous structures. CN117936755A discloses a method for improving the conductivity and rate performance of NFPP positive electrode materials using a double carbon coating structure. The structure and performance of the positive electrode material can be further optimized by pre-carbonizing the sodium source and rationally selecting the type of iron source / sodium source carbon source. The specific range of preparation process parameters, such as temperature, time, rotation speed, etc., is given to provide a reference for industrial production. The test results of the embodiment show that the NFPP positive electrode material prepared by this method has a high discharge specific capacity, which is close to the theoretical value. However, it needs to be prepared through multiple steps, such as dissolution, drying, roasting, ball milling, spray drying, calcination, etc., and the process route is relatively complicated. In addition, expensive alcohol solvents (such as ethanol) are used for wet ball milling, which is relatively costly and requires some steps, such as roasting and calcining, to be performed under an inert atmosphere, which places high demands on equipment.

[0007] CN 117776138A discloses a method for preparing NFPP positive electrode material using a soft template method, which can form NFPP crystal nuclei on the template, and at the same time, PAM decomposes at high temperature to form a carbon coating on the crystal nuclei. This carbon coating structure can shorten the ion transmission distance, improve the ion transmission efficiency, and thus improve the conductivity of the positive electrode material. However, the raw material cost is high. This method uses polyacrylamide (PAM) as a soft template. PAM is more expensive than other template materials, which may increase production costs. At the same time, the energy consumption is high. This method requires high-temperature calcination (500°C) for up to 8-15 hours, which consumes a lot of energy and increases production energy consumption.

[0008] Although the above methods have improved the electrochemical performance of NFPP from different perspectives, most of them have defects such as complex process, high energy consumption, and difficulty in scale-up production, which hinder the actual commercial application of NFPP. Therefore, it is particularly urgent and important to develop a simple, low-energy, and easy-to-scale NFPP synthesis method.

[0009] In summary, sodium-ion batteries are considered to be a promising new energy storage system after lithium-ion batteries due to their abundant resource reserves, low cost and environmental friendliness. As a key positive electrode material, NFPP has unique advantages such as high theoretical specific capacity, moderate average operating voltage and stable structure, but its poor electronic conductivity and ion diffusion restrict its practical application. Developing a simple, efficient and easy-to-scale NFPP synthesis method is of great significance to promote the practical application of sodium-ion batteries. Summary of the invention

[0010] The present invention hopes to provide a method for preparing NFPP material as a positive electrode material for sodium ion batteries by a dual organic molecular template method. The specific scheme is as follows:

[0011] A method for preparing NFPP material as a positive electrode material for a sodium ion battery by a dual organic molecular template method, characterized in that it comprises the following steps:

[0012] (1) adding an alkali metal source, an iron source, a phosphate source and a doping element source to a solvent in sequence and stirring;

[0013] (2) adding two different complexing agents;

[0014] (3) Two-step stirring: first step: stirring at 50-60° C. for 10-20 minutes, second step: stirring at 70-80° C. for 30-40 minutes;

[0015] (4) continuously stirring until a gel-like precursor is formed;

[0016] (5) Drying treatment: transferring the precursor into a vacuum oven;

[0017] (6) High temperature calcination: Place the dried sample in a tubular furnace and perform two-stage calcination in an inert gas atmosphere: The first stage: 300-400°C, keep warm for 2-4 hours, and increase the temperature by 3-5°C / min. The second stage: 450-550°C, keep warm for 4-6 hours, and increase the temperature by 3-5°C / min. After calcination, cool the sample in the furnace.

[0018] (7) Screening treatment: the cooled sintered product is screened through a 50-100 mesh screen to obtain a positive electrode material for a sodium ion battery;

[0019] The general structural formula of the positive electrode material of the sodium ion battery is Na4Fe 3-x B x (PO4)2P2O7 / C, wherein the x of the doping element B ranges from 0 to 0.3.

[0020] The complexing agent in step (2) is at least two of citric acid, glucose, glycine, alanine and glutamic acid, and the mass ratio of the two complexing agents is 1:1 to 1:3.

[0021] The doping element source in step (1) is at least one of Al, Mn and Ti.

[0022] The inert gas in step (6) is at least one of argon, nitrogen or helium, and the gas flow rate is 50-100 ml / min.

[0023] After the high temperature calcination in step (6), a low temperature annealing treatment is performed, the annealing temperature is 200-300° C., and the time is 2-6 hours.

[0024] The oven temperature of step (5) is 75-85° C., and the baking time is 8-14 hours.

[0025] The method optimizes the thickness of the carbon coating layer of the NFPP composite material by regulating the ratio of two organic small molecule complexing agents, so that the thickness of the carbon coating layer is controlled within the range of 2-10 nm.

[0026] The method of the invention adopts an aqueous solution system, avoids the use of organic solvents, and the reaction temperature does not exceed 600° C. during the entire preparation process.

[0027] Button battery production: The modified polyanion mixed phosphoric acid system positive electrode material obtained above is assembled into a button battery. The prepared positive electrode material, conductive agent (acetylene black) and binder (polyvinylidene fluoride PVDF, pre-prepared into an NMP solution containing 8wt% of PVDF) are weighed in a mass ratio of 80:10:10 and fully ground and mixed. N-methylpyrrolidone (NMP) is used as a dispersant to adjust it into a slurry of a certain viscosity. The obtained slurry is evenly coated on aluminum foil, and after vacuum drying and stamping, a positive electrode sheet is made. A disc-shaped high-purity metal sodium sheet is used as the negative electrode. The electrolyte is an organic solution of 1mol / LNaClO4 (EC / DMC=1 / 1, v / v), and the battery separator is a glass fiber filter paper. The button battery assembly is completed in a glove box under an argon atmosphere.

[0028] The difference between the present invention and the background technology is that the carbon-coated modified polyanion mixed phosphoric acid system positive electrode material is prepared by using a dual organic molecular template induction and a sol-gel method. This scheme is the first to use a dual complexation method to construct a carbon three-dimensional grid structure to coat the modified polyanion mixed phosphoric acid system to construct a positive electrode material. Usually, a single complexing agent is used to adjust the microstructure of the modified polyanion mixed phosphoric acid system positive electrode material, which has been shown to have limited improvement in electrochemical performance, especially rate capability. The reason for these unsatisfactory modification effects may be that a single organic acid has a high affinity for organic molecules and Fe. 2+ The regulatory capacity for forming moderate interactions between ions is quite limited. In addition, when the carbon species from a single carbon source are in the nucleation stage, they have a large surface Gibbs free energy. This state inevitably leads to thermodynamic agglomeration at high temperatures, making it difficult to adjust the uniformity and thickness of the carbon layer. Unlike the commonly used process based on a single complexing agent, the carefully designed dual complexing agent system has obvious advantages in improving the microstructure and electrochemical properties of the modified polyanion mixed phosphoric acid system. The hydrophilic bond between the two complexing agents in the aqueous solution is utilized to capture the free anions and cations by the end groups, controlling the growth of the grain size. The heterogeneous three-dimensional network structure formed by their combination is conducive to a more uniform and controllable thickness of the conductive carbon layer on the surface of the modified polyanion mixed phosphoric acid system after calcination.

[0029] The innovation of the present invention lies in: proposing a new strategy of synergistic coordination of citric acid and glycine dual ligands, and intending to optimize the microstructure of NFPP through the synergistic effect between the two ligands. The dual ligand system has unique advantages: glycine reduces the viscosity of the solution and promotes ion diffusion; the two ligands form a three-dimensional network that is conducive to the formation of a uniform carbon coating layer. By regulating the feed ratio of the two ligands, an optimized NFPP composite material is obtained, showing excellent microstructures such as reduced particle size, good dispersibility, and a moderate carbon coating layer (~2nm). The NFPP electrode shows excellent sodium storage performance, such as high reversible capacity, good cycle stability, and excellent rate performance, which confirms the superiority of the dual ligand strategy. The dual complexing agent described in the present invention is used to prepare a modified polyanion mixed phosphoric acid system positive electrode material. The dual complexing agent can be directly prepared by mixing the materials, drying them, and then calcining them to obtain a carbon-coated sodium iron phosphate pyrophosphate composite material. The preparation method is simple and suitable for industrial production.

[0030] The present invention proposes an innovative dual organic molecular template induction method for preparing a modified polyanion mixed phosphate system positive electrode material. This method cleverly combines the sol-gel method and high-temperature sintering technology to obtain a high-performance positive electrode material with uniform carbon coating. The core innovation of the present invention lies in the use of two different organic small molecules as complexing agents, which can be citric acid, glucose or amino acid substances. This dual complexing agent system can accurately control the growth process of the material at the molecular level to form a unique three-dimensional network structure. In the subsequent high-temperature treatment process, these organic small molecules will decompose and form a uniform carbon coating layer in situ. Through this dual organic molecular template induction strategy, the present invention achieves the following key advantages: Particle size control: The dual complexing agent system can effectively control the growth of positive electrode material particles, making the particle size distribution of the final product more uniform, which is conducive to improving the electrochemical performance of the material. Carbon coating optimization: The carbon layer formed by the decomposition of organic small molecules at high temperature has a uniform thickness, and the coating is more complete, which significantly improves the conductivity of the material. Structural stability: The three-dimensional network structure formed by the dual complexing agent helps to maintain the structural stability of the material during the charging and discharging process, reduce volume changes, and extend battery life. Improved capacity density: By optimizing the microstructure and conductivity of the material, the cathode material prepared by this method has a higher capacity density. Enhanced electrochemical performance: The uniform carbon coating and optimized microstructure work together to significantly improve the electronic conductivity and ion diffusion rate of the material, thereby comprehensively improving the electrochemical performance of the cathode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a process flow chart of a dual organic molecular template-induced NFPP conductive carbon mesoporous nanocomposite of the present invention;

[0032] Figure 2 The composite material Na4Fe2.8 Ti 0.2 SEM image of (PO4)2P2O7@C0.2 C;

[0033] Figure 3 The composite material Na4Fe 2.8 Ti 0.2 Discharge specific capacity diagram of (PO4)2P2O7@C0.2 C;

[0034] Figure 4 It is a cycle performance diagram of 300 cycles at 1C for Example 4, Example 5 and Example 6. DETAILED DESCRIPTION

[0035] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments in this application can be combined with each other. In order to further understand the present invention, the present invention is further described below in conjunction with the specification and specific preferred embodiments, and these embodiments cannot be understood as limiting the scope of protection claimed in this application.

[0036] Example 1

[0037] This embodiment provides a method for modifying a polyanion mixed phosphate system positive electrode material by inducing dual organic molecular templates, and in the embodiment, glycine and citric acid are used as complexing agents as examples, and the method is as follows:

[0038] First, weigh 0.2 mol sodium pyrophosphate, 0.6 mol ferrous oxalate, and 0.4 mol ammonium dihydrogen phosphate, add them to a beaker containing a solvent, stir at 50°C for 15 minutes, then add 0.5 mol glycine and 0.2 mol citric acid in turn, continue stirring at 70°C until the solution becomes a gel, and use deionized water as the solvent. Transfer the gel solid to a vacuum oven for further baking for 12 hours, and set the oven temperature to 80°C. The precursor sample is first heated to 350°C at a rate of 5°C / min in a nitrogen atmosphere for 3 hours, and then heated to 550°C at a rate of 5°C / min for secondary sintering for 5 hours. High-purity nitrogen (≥99.99%) is continuously introduced during the whole process; after the secondary sintering is completed, it is cooled to room temperature with the furnace, and the solid product is sieved through a 100-mesh sieve to obtain the composite material Na4Fe3(PO4)2P2O7@C.

[0039] The sodium ion battery modified polyanion positive electrode material prepared in this embodiment is used to assemble a button cell using a sodium sheet as a counter electrode. The discharge specific capacity at 0.2C current is as high as 90mAh / g, and the capacity retention rate is more than 96% after 300 discharge cycles at 1C rate.

[0040] Example 2

[0041] Compared with Example 1, the only difference is that the ratio of glycine to citric acid is increased to 5:1, as follows:

[0042] First, weigh 0.2 mol sodium pyrophosphate, 0.6 mol ferrous oxalate, and 0.4 mol ammonium dihydrogen phosphate, add them to a beaker containing a solvent, stir at 50°C for 15 minutes, then add 1 mol glycine and 0.2 mol citric acid in turn, continue stirring at 70°C until the solution becomes a gel, and use deionized water as the solvent. Transfer the gel solid to a vacuum oven for further baking for 12 hours, and set the oven temperature to 80°C. The precursor sample is first heated to 350°C at a rate of 5°C / min in a nitrogen atmosphere for 3 hours, and then heated to 550°C at a rate of 5°C / min for secondary sintering for 5 hours. High-purity nitrogen (≥99.99%) is continuously introduced during the whole process; after the secondary sintering is completed, it is cooled to room temperature with the furnace, and the obtained solid product is sieved through a 100-mesh sieve to obtain the composite material Na4Fe3(PO4)2P2O7@C.

[0043] The sodium ion battery modified polyanion positive electrode material prepared in this embodiment is used to assemble a button cell using a sodium sheet as a counter electrode. The discharge specific capacity at 0.2C current is as high as 97mAh / g, and the capacity retention rate is more than 98% after 300 discharge cycles at 1C rate.

[0044] Example 3

[0045] Compared with Example 1, the only difference is that the ratio of glycine to citric acid is increased to 10:1, as follows:

[0046] First, weigh 0.2 mol sodium pyrophosphate, 0.6 mol ferrous oxalate, and 0.4 mol ammonium dihydrogen phosphate, add them to a beaker containing a solvent, stir at 50°C for 15 minutes, then add 2 mol glycine and 0.2 mol citric acid in turn, continue stirring at 70°C until the solution becomes a gel, and use deionized water as the solvent. The gel-like solid is transferred to a vacuum oven for further baking for 12 hours, and the oven temperature is set to 80°C. The precursor sample is first heated to 350°C at a rate of 5°C / min in a nitrogen atmosphere for sintering for 3 hours, and then heated to 550°C at a rate of 5°C / min for secondary sintering for 5 hours. High-purity nitrogen (≥99.99%) is continuously introduced during the whole process; after the secondary sintering is completed, it is cooled to room temperature with the furnace, and the solid product is sieved through a 100-mesh sieve to obtain the composite material Na4Fe3(PO4)2P2O7@C.

[0047] The sodium ion battery modified polyanion positive electrode material prepared in this embodiment is used to assemble a button cell using a sodium sheet as a counter electrode. The discharge specific capacity at 0.2C current is as high as 93mAh / g, and the capacity retention rate is more than 97% after 300 discharge cycles at 1C rate.

[0048] Example 4

[0049] Compared with Example 2, the only difference is that titanium is added as a doping element, as follows:

[0050] First, weigh 0.2 mol of sodium pyrophosphate, 0.56 mol of ferrous oxalate, 0.4 mol of ammonium dihydrogen phosphate, and 0.04 mol of titanium dioxide, add them to a beaker containing a solvent, stir at 50°C for 15 minutes, then add 1 mol of glycine and 0.2 mol of citric acid in turn, and continue stirring at 70°C until the solution becomes a gel, with deionized water as the solvent. The gel-like solid is transferred to a vacuum oven for further baking for 12 hours, and the oven temperature is set to 80°C. The precursor sample is first heated to 350°C at a rate of 5°C / min in a nitrogen atmosphere and sintered for 3 hours, and then heated to 550°C at a rate of 5°C / min for a secondary sintering for 5 hours. High-purity nitrogen (≥99.99%) is continuously introduced during the whole process; after the secondary sintering is completed, it is cooled to room temperature with the furnace, and the obtained solid product is sieved through a 100-mesh sieve to obtain the composite material Na4Fe 2.8 Ti 0.2 (PO4)2P2O7@C.

[0051] The sodium ion battery modified polyanion positive electrode material prepared in this embodiment is used to assemble a button cell using a sodium sheet as a counter electrode. The discharge specific capacity at 0.2C current is as high as 113 mAh / g, and the capacity retention rate is more than 97% after 300 discharge cycles at 1C rate.

[0052] Example 5

[0053] Compared with Example 2, the only difference is that manganese is added as a doping element, as follows:

[0054] First, weigh 0.2 mol of sodium pyrophosphate, 0.56 mol of ferrous oxalate, 0.4 mol of ammonium dihydrogen phosphate, and 0.04 mol of manganese oxalate, add them to a beaker containing a solvent, stir at 50°C for 15 minutes, then add 1 mol of glycine and 0.2 mol of citric acid in turn, and continue stirring at 70°C until the solution becomes a gel, with deionized water as the solvent. The gel-like solid is transferred to a vacuum oven for further baking for 12 hours, and the oven temperature is set to 80°C. The precursor sample is first heated to 350°C at a rate of 5°C / min in a nitrogen atmosphere and sintered for 3 hours, and then heated to 550°C at a rate of 5°C / min for a secondary sintering for 5 hours. High-purity nitrogen (≥99.99%) is continuously introduced during the whole process; after the secondary sintering is completed, it is cooled to room temperature with the furnace, and the obtained solid product is sieved through a 100-mesh sieve to obtain the composite material Na4Fe 2.8 Mn 0.2 (PO4)2P2O7@C.

[0055] The sodium ion battery modified polyanion positive electrode material prepared in this embodiment is used to assemble a button cell using a sodium sheet as a counter electrode. The discharge specific capacity at 0.2C current is as high as 104mAh / g, and the capacity retention rate is more than 93% after 300 discharge cycles at 1C rate.

[0056] Example 6

[0057] Compared with Example 2, the only difference is that aluminum is added as a doping element, as follows:

[0058] First, weigh 0.2 mol of sodium pyrophosphate, 0.546 mol of ferrous oxalate, 0.4 mol of ammonium dihydrogen phosphate, and 0.04 mol of aluminum dihydrogen phosphate, add them to a beaker containing a solvent, stir at 50°C for 15 minutes, then add 1 mol of glycine and 0.2 mol of citric acid in turn, and continue stirring at 70°C until the solution becomes a gel, with deionized water as the solvent. The gel-like solid is transferred to a vacuum oven for further baking for 12 hours, and the oven temperature is set to 80°C. The precursor sample is first heated to 350°C at a rate of 5°C / min in a nitrogen atmosphere and sintered for 3 hours, and then heated to 550°C at a rate of 5°C / min for a secondary sintering for 5 hours. High-purity nitrogen (≥99.99%) is continuously introduced during the whole process; after the secondary sintering is completed, it is cooled to room temperature with the furnace, and the resulting solid product is sieved through a 100-mesh sieve to obtain the composite material Na4Fe 2.7 Al 0.2 (PO4)2P2O7@C. The sodium ion battery modified polyanion positive electrode material prepared in this embodiment is used to assemble a button cell using a sodium sheet as a counter electrode. The discharge capacity at 0.2C current is as high as 102 mAh / g, and the capacity retention rate after 300 cycles at 1C rate is more than 95%.

[0059] Comparative Example 1

[0060] Compared with Example 1, the only difference is that glycine and citric acid are not used, and the details are as follows:

[0061] First, weigh 0.2 mol of sodium pyrophosphate, 0.6 mol of ferrous oxalate, and 0.4 mol of ammonium dihydrogen phosphate, add them to a beaker containing a solvent, and stir at 50°C for 15 minutes until the solution becomes a gel, with deionized water as the solvent. Transfer the gel-like solid to a vacuum oven for further baking for 12 hours, and set the oven temperature to 80°C. The precursor sample is first heated to 350°C at a rate of 5°C / min in a nitrogen atmosphere for sintering for 3 hours, and then heated to 550°C at a rate of 5°C / min for secondary sintering for 5 hours. High-purity nitrogen (≥99.99%) is continuously introduced during the whole process; after the secondary sintering is completed, it is cooled to room temperature with the furnace, and the solid product is sieved through a 100-mesh sieve to obtain the composite material Na4Fe3(PO4)2P2O7.

[0062] The sodium ion battery modified polyanion positive electrode material prepared in this comparative example is used to assemble a button cell using a sodium sheet as a counter electrode. The discharge specific capacity at 0.2C current is as high as 77mAh / g, and the capacity retention rate is more than 85% after 300 discharge cycles at 1C rate.

[0063] Comparative Example 2

[0064] Compared with Example 1, the only difference is that glycine is not used, and the details are as follows:

[0065] First, weigh 0.2 mol sodium pyrophosphate, 0.6 mol ferrous oxalate, and 0.4 mol ammonium dihydrogen phosphate, add them to a beaker containing a solvent, stir at 50°C for 15 minutes, then add 1.2 mol citric acid in turn, continue stirring at 70°C until the solution becomes a gel, and use deionized water as the solvent. Transfer the gel solid to a vacuum oven for further baking for 12 hours, and set the oven temperature to 80°C. The precursor sample is first heated to 350°C at a rate of 5°C / min in a nitrogen atmosphere for sintering for 3 hours, and then heated to 550°C at a rate of 5°C / min for secondary sintering for 5 hours. High-purity nitrogen (≥99.99%) is continuously introduced during the whole process; after the secondary sintering is completed, it is cooled to room temperature with the furnace, and the solid product is sieved through a 100-mesh sieve to obtain the composite material Na4Fe3(PO4)2P2O7@C.

[0066] The sodium ion battery modified polyanion positive electrode material prepared in this comparative example is used to assemble a button cell using a sodium sheet as a counter electrode. The discharge specific capacity at 0.2C current is as high as 83mAh / g, and the capacity retention rate is more than 89% after 300 discharge cycles at 1C rate.

[0067] Comparative Example 3

[0068] Compared with Example 1, the only difference is that citric acid is not used, specifically as follows:

[0069] First, weigh 0.2 mol sodium pyrophosphate, 0.6 mol ferrous oxalate, and 0.4 mol ammonium dihydrogen phosphate, add them to a beaker containing a solvent, stir at 50°C for 15 minutes, then add 1.2 mol glycine in turn, continue stirring at 70°C until the solution becomes a gel, and use deionized water as the solvent. Transfer the gel solid to a vacuum oven for further baking for 12 hours, and set the oven temperature to 80°C. The precursor sample is first heated to 350°C at a rate of 5°C / min in a nitrogen atmosphere for 3 hours, and then heated to 550°C at a rate of 5°C / min for secondary sintering for 5 hours. High-purity nitrogen (≥99.99%) is continuously introduced during the whole process; after the secondary sintering is completed, it is cooled to room temperature with the furnace, and the obtained solid product is sieved through a 100-mesh sieve to obtain the composite material Na4Fe3(PO4)2P2O7@C.

[0070] The sodium ion battery modified polyanion positive electrode material prepared in this comparative example is used to assemble a button cell using a sodium sheet as a counter electrode. The discharge specific capacity at 0.2C current is as high as 89mAh / g, and the capacity retention rate is more than 89% after 300 discharge cycles at 1C rate.

[0071] Table 1 Parameters and performance comparison of each embodiment and comparative example

[0072] Experimental protocol Glycine:Citrate Doping elements <![CDATA[0.2 C capacity / mAh·g -1 > 1C capacity retention rate Example 1 2.5∶1 / 90 300 laps 96% Example 2 5∶1 / 97 300 laps 98% Example 3 10∶1 / 93 300 laps 97% Example 4 5∶1 Ti 113 300 laps 97% Example 5 5∶1 Mn 104 300 laps 93% Example 6 5∶1 Al 102 300 laps 95% Comparative Example 1 / / 77 300 laps 85% Comparative Example 2 Use only citric acid / 83 300 laps 89% Comparative Example 3 Only glycine is used / 89 300 laps 89%

[0073] The embodiments described above are only some examples of the present invention, rather than all the embodiments, and are not intended to limit the protection scope of the present invention.

Claims

1. A method for preparing NFPP material as a positive electrode material for sodium ion batteries by a dual organic molecular template method. It is characterized in that The following steps are involved: (1) adding an alkali metal source, an iron source, a phosphate source and a doping element source to a solvent in sequence and stirring; (2) adding two different complexing agents; (3) Two-step stirring: first step: stirring at 50-60° C. for 10-20 minutes, second step: stirring at 70-80° C. for 30-40 minutes; (4) continuously stirring until a gel-like precursor is formed; (5) Drying treatment: transferring the precursor into a vacuum oven; (6) High temperature calcination: Place the dried sample in a tubular furnace and perform two-stage calcination in an inert gas atmosphere: The first stage: 300-400°C, keep warm for 2-4 hours, and increase the temperature by 3-5°C / min. The second stage: 450-550°C, keep warm for 4-6 hours, and increase the temperature by 3-5°C / min. After calcination, cool the sample in the furnace. (7) Screening treatment: the cooled sintered product is screened through a 50-100 mesh screen to obtain a positive electrode material for a sodium ion battery; The general structural formula of the positive electrode material of the sodium ion battery is Na 4 Fe 3-x B x (PO 4 ) 2 P 2 O 7 / C, wherein the x range of the doping element B is 0 to 0.

3.

2. A method for preparing NFPP material as a positive electrode material for sodium ion batteries by a dual organic molecular template method as claimed in claim 1, Features: The complexing agent in step (2) is at least two of citric acid, glucose, glycine, alanine and glutamic acid, and the mass ratio of the two complexing agents is 1:1 to 1:

3.

3. A method for preparing NFPP material as a positive electrode material for sodium ion batteries by a dual organic molecular template method as claimed in claim 1, It is characterized in that The doping element source in step (1) is at least one of Al, Mn and Ti.

4. A method for preparing NFPP material as a positive electrode material for sodium ion batteries by a dual organic molecular template method as claimed in claim 1, Features: The inert gas in step (6) is at least one of argon, nitrogen or helium, and the gas flow rate is 50-100 ml / min.

5. A method for preparing NFPP material as a positive electrode material for sodium ion batteries by a dual organic molecular template method as claimed in claim 1, It is characterized in that After the high temperature calcination in step (6), a low temperature annealing treatment is performed, the annealing temperature is 200-300° C., and the time is 2-6 hours.

6. A method for preparing NFPP material as a positive electrode material for sodium ion batteries by a dual organic molecular template method as claimed in claim 1, It is characterized in that The oven temperature of step (5) is 75-85° C., and the baking time is 8-14 hours.

Citation Information

Patent Citations

  • Positive electrode material for sodium-ion battery and preparation method thereof

    CN108046231A

  • Sodium-iron double-doped polyanion positive electrode material and preparation method thereof

    CN117558905A

Cited By

  • Preparation method of soft template method sodium ion battery fluoro-iron-based polyanionic positive electrode material and fluoro-iron-based polyanionic positive electrode material

    CN121812511A