Silicon-carbon composite material as well as preparation method and application thereof
Through the preparation method of silicon-carbon composite materials, a unique pore structure and carbon cladding layer is formed using template agents and pore-forming agents, which solves the problems of pole sheet shedding and battery performance degradation caused by changes in the volume of silicon negative electrodes, and improves the ratio of lithium-ion batteries Capacity and cycling performance.
Patent Information
- Application Number
- CN202410876815.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-11-08
AI Technical Summary
The volume of the silicon negative electrode changes greatly during the lithium embedding and deliquification process, resulting in the problem of the electrode sheet falling off, the electrode powdering, and the battery circulation performance deterioration.
Using the preparation method of silicon-carbon composite materials, a unique pore structure is formed by mixing and sintering the silicon source, carbon source, template agent and pore-forming agent to sinter a unique pore structure, alleviating the change in silicon volume, and generating a carbon cladding layer in situ to increase the silicon load. quantity and conductivity.
Effectively buffer the expansion and contraction of silicon, improve the specific capacity, first effect and circulation performance of lithium-ion batteries, avoid the shedding of the electrode sheet and the powdering of the electrode, and achieve high specific capacity and excellent circulation performance.
Smart Images

Figure CN118908176A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of negative electrode material preparation, and specifically relates to a silicon-carbon composite material and a preparation method and application thereof. Background Art
[0002] Fossil energy is an important energy and material basis for us, and is inseparable from human development. However, the use of fossil energy not only brings serious environmental pollution, but also puts fossil energy at risk of depletion. Therefore, it is imperative to develop clean and sustainable new energy.
[0003] Lithium-ion batteries are currently the most successful form of new energy and have been widely used in electric vehicles, portable appliances, large-scale energy storage and other fields; they have relatively high energy density, long cycle life and relatively reliable safety. Commercial graphite is currently the commonly used negative electrode material for lithium-ion batteries, and its theoretical specific capacity is 372mAh / g. Graphite negative electrodes have the advantages of good stability and small volume expansion; but their specific capacity is low, making it difficult to further improve the battery energy density.
[0004] The theoretical specific capacity of silicon is 4200mAh / g, which is more than ten times that of graphite. Therefore, silicon has become the preferred negative electrode material for the development of high energy density batteries. However, silicon negative electrodes have the following problems: 1) During the process of lithium insertion and removal, the volume of silicon expands and contracts greatly, such as a maximum expansion of 300%, causing the pole piece to fall off, the electrode to pulverize, and the battery cycle performance to decline rapidly; 2) Silicon is a semiconductor with poor intrinsic conductivity. Summary of the invention
[0005] Therefore, the technical problem to be solved by the present invention is to overcome the problems in the prior art that the volume of silicon changes greatly during the lithium insertion and removal process, resulting in the falling off of the pole pieces, electrode pulverization, and decreased electrical performance of the battery, thereby providing a silicon-carbon composite material and its preparation method and application.
[0006] To this end, the present invention provides the following technical solutions.
[0007] The present invention provides a method for preparing a silicon-carbon composite material, comprising the following steps: mixing a silicon source, a carbon source, a template agent and a pore-forming agent, and sintering;
[0008] Wherein, the template agent is at least one of nano magnesium oxide, nano zinc oxide, nano calcium carbonate, sodium chloride, potassium chloride and calcium chloride;
[0009] The pore-forming agent is potassium hydroxide or phosphoric acid solution.
[0010] In an optional embodiment, the template is at least two of nano magnesium oxide, nano zinc oxide, nano calcium carbonate, sodium chloride, potassium chloride and calcium chloride;
[0011] In an optional embodiment, the pore former is a phosphoric acid solution.
[0012] In an optional embodiment, the template includes calcium chloride and nano zinc oxide;
[0013] In an optional embodiment, the concentration of the phosphoric acid solution is not less than 85 wt %.
[0014] In an optional embodiment, the mass ratio of the template to the pore-forming agent is (3-60): (12-50).
[0015] In an optional embodiment, the mixing step further comprises the step of adding a heteroatom precursor;
[0016] Preferably, the heteroatom precursor is a nitrogen-containing compound;
[0017] Preferably, the heteroatom precursor is at least one of melamine, ammonia, urea, thiourea and ammonium hydrogen phosphate;
[0018] Preferably, the mass ratio of the heteroatom precursor to the template is (3-35):(3-60).
[0019] In an optional embodiment, the mass ratio of the silicon source, the carbon source, and the template is (5-50): (2-40): (3-60);
[0020] Preferably, the carbon source is at least one of petroleum asphalt, glucose, coal thermal catalytic heavy components, lignin, phenolic resin, epoxy resin and polyacrylonitrile;
[0021] Preferably, the silicon source is at least one of nano-silicon, micro-silicon and porous silicon;
[0022] Preferably, the particle size of the nano-silicon is 20-500nm;
[0023] Preferably, the particle size of the micron silicon is 1-50 μm.
[0024] In an optional embodiment, the specific steps of sintering include: heating to 350-1200° C. at a heating rate of 0.5-20° C. / min and then keeping the temperature for 0.1-20 h;
[0025] Preferably, the sintering is carried out under a protective atmosphere;
[0026] Preferably, the protective atmosphere comprises at least one of an inert gas and nitrogen;
[0027] Preferably, during the sintering, the flow rate of the protective atmosphere is 30-500 ml / min.
[0028] In an optional embodiment, the sintering further includes a pickling step;
[0029] Preferably, the pickling solution for pickling is at least one of hydrochloric acid, nitric acid and sulfuric acid;
[0030] Preferably, the concentration of the pickling solution is 1-3 mol / L.
[0031] The present invention provides a silicon-carbon composite material prepared by the above preparation method.
[0032] The present invention provides an application of the silicon-carbon composite material prepared by the above preparation method in pole pieces and / or lithium-ion batteries.
[0033] The technical solution of the present invention has the following advantages:
[0034] 1. The preparation method of the silicon-carbon composite material provided by the present invention comprises mixing a silicon source, a carbon source, a template agent and a pore-forming agent, and sintering; wherein the template agent is at least one of nano magnesium oxide, nano zinc oxide, nano calcium carbonate, sodium chloride, potassium chloride and calcium chloride; and the pore-forming agent is potassium hydroxide or phosphoric acid. The silicon-carbon composite material prepared by the preparation method can form a unique pore structure, such as having a special surface area, pore volume and pore size distribution, which greatly alleviates the volume change of silicon. The silicon content in the composite material is high. The silicon negative electrode in the prior art produces a large volume expansion during the lithium insertion process, and partially shrinks after lithium removal. Repeated expansion and contraction causes the electrode material to pulverize, fall off, and the cycle performance deteriorates. When the silicon-carbon composite material prepared by the present invention is applied to a pole piece or a battery, it has a buffering effect on the expansion and contraction, and there will be no problems of pole piece falling off, electrode pulverization and battery performance degradation, so that the battery has a high specific capacity, high initial efficiency and excellent cycle performance. Specifically, the present invention adopts a template and a pore-forming agent in combination, with at least one of nano magnesium oxide, nano zinc oxide, nano calcium carbonate, sodium chloride, potassium chloride and calcium chloride as the template, and potassium hydroxide or phosphoric acid as the pore-forming agent, which can effectively adjust the pore size, pore structure and specific surface area of the silicon-carbon composite material. The use of silicon-carbon materials in lithium-ion batteries can regulate the transmission channels of lithium ions and electrons, greatly buffer the volume changes of silicon, such as expansion or contraction, and improve the specific capacity, initial efficiency and cycle performance of lithium-ion batteries.
[0035] Furthermore, the silicon-carbon composite material prepared by the method of in-situ generation of the carbon coating layer of the present invention is carbon-coated silicon, which can make the silicon dispersed more evenly in the carbon coating, not easy to agglomerate during the preparation process, and can increase the silicon loading amount. When the silicon-carbon composite material is applied to the battery, the electrical performance, such as specific capacity, first efficiency and cycle performance, can be further improved. In addition, the method of the present invention is also simple in process, easy to scale up and industrialized.
[0036] 2. In the preparation method of the silicon-carbon composite material provided by the present invention, the template agent is at least two of nano-magnesium oxide, nano-zinc oxide, nano-calcium carbonate, sodium chloride, potassium chloride and calcium chloride, and calcium chloride and nano-zinc oxide are preferably used as the composite template agent, which helps to further improve the performance of the silicon-carbon material and prevent the problem of large volume changes in silicon.
[0037] 3. The preparation method of the silicon-carbon composite material provided by the present invention uses a nitrogen-containing compound as a raw material, which can improve the conductivity of the silicon-carbon composite material, thereby improving its lithium storage electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0039] Figure 1 is the thermogravimetric analysis result of the silicon-carbon composite material prepared in Example 1 of the present invention;
[0040] Figure 2 This is a high-resolution transmission electron microscope image of the silicon-carbon composite material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0041] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0042] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0043] The method for preparing the coal thermal dissolution catalytic heavy component is disclosed in patent CN100547055C, wherein the coal thermal dissolution catalytic heavy component used in the following examples and comparative examples is prepared with reference to Example 1 in patent CN100547055C.
[0044] Example 1
[0045] This embodiment provides a method for preparing a silicon-carbon composite material, which specifically includes the following steps:
[0046] 1) 25.0 g of silicon powder (150 nm), 5.0 g of coal hot-dissolving catalytic heavy components, 6.8 g of calcium chloride, 5.0 g of nano zinc oxide, 15.3 g of phosphoric acid solution (the concentration of the phosphoric acid solution is 85 wt%), and 6.0 g of thiourea are crushed and mixed, and ball-milled in a high-energy ball mill for 1 hour. The treated powder is placed in a boat, and the boat is placed in a tube furnace.
[0047] 2) In a nitrogen atmosphere, the nitrogen flow rate is 150 ml / min; the tube furnace is heated to 850°C at a heating rate of 3°C / min and maintained for 2.5 hours, and then cooled to room temperature to obtain a silicon-carbon precursor; the silicon-carbon precursor powder is mixed with an HCl solution (the concentration of the HCl solution is 2M, and the amount added is 80 ml), stirred at 80°C for 8 hours, and then washed with deionized water to a pH of 7.0, and then vacuum dried at 110°C for 24 hours to obtain the silicon-carbon composite material.
[0048] The specific surface area of the silicon-carbon composite material obtained in the above embodiment is 66.2 m 2 / g, pore volume is 0.23cm 3 / g, and the average pore size is 10.5nm. Figure 1 The thermogravimetric analysis result of the silicon-carbon composite material prepared in Example 1 shows that the silicon content is 91.8wt%. The XPS analysis result shows that the nitrogen content is 0.95at%. Figure 2 This is a high-resolution transmission electron micrograph of the silicon-carbon composite material obtained in Example 1. It is observed that the composite material has a silicon crystal core and an outer layer covered by amorphous carbon with a thickness of about 9 nm.
[0049] Example 2
[0050] This embodiment provides a method for preparing a silicon-carbon composite material, which specifically includes the following steps:
[0051] 1) 6.0 g of silicon powder (100 nm), 6.8 g of coal hot-dissolving catalytic heavy components, 16.8 g of sodium chloride, 7.0 g of nano-magnesium oxide, 22.1 g of phosphoric acid solution (the concentration of the phosphoric acid solution is 85 wt%), and 4.5 g of melamine are crushed and mixed, and ball-milled in a high-energy ball mill for 1 hour. The treated powder is placed in a boat, and the boat is placed in a tube furnace.
[0052] 2) In a nitrogen atmosphere, the nitrogen flow rate is 150 ml / min; the tubular furnace is heated to 1050°C at a heating rate of 2°C / min and maintained for 2.0 hours, and then cooled to room temperature to obtain a silicon-carbon precursor; the silicon-carbon precursor powder is mixed with an HCl solution (the concentration of the HCl solution is 2M, and the amount added is 200 ml), stirred at 80°C for a total stirring time of 8 hours, and then washed with deionized water to a pH of 7.0, and then vacuum dried at 110°C for 24 hours to obtain the silicon-carbon composite material.
[0053] The specific surface area of the silicon-carbon composite material obtained in the above embodiment is 58.2 m 2 / g, pore volume is 0.24cm 3 / g, and the average pore size is 9.5nm. Thermogravimetric analysis results of the prepared silicon-carbon composite material show that the silicon content is 90.3wt%. According to the XPS analysis results, the nitrogen content is 1.25at%.
[0054] Example 3
[0055] This embodiment provides a method for preparing a silicon-carbon composite material, which specifically includes the following steps:
[0056] 1) 12.0 g of silicon powder (50 nm), 3.5 g of lignin, 11.2 g of potassium chloride, 4.5 g of nano zinc oxide, 19.9 g of phosphoric acid solution (the concentration of the phosphoric acid solution is 85 wt%), and 7.1 g of urea are ground and mixed, and ball-milled in a high-energy ball mill for 1 hour. The processed powder is placed in a boat, and the boat is placed in a tube furnace.
[0057] 2) In a nitrogen atmosphere, the nitrogen flow rate is 200 ml / min; the tubular furnace is heated to 950°C at a heating rate of 3°C / min and maintained for 3.0 hours, and then cooled to room temperature to obtain a silicon-carbon precursor; the silicon-carbon precursor powder is mixed with an HCl solution (the concentration of the HCl solution is 2M, and the amount added is 70 ml), stirred at 80°C for a total stirring time of 8 hours, and then washed with deionized water to a pH of 7.0, and then vacuum dried at 110°C for 24 hours to obtain the silicon-carbon composite material.
[0058] The specific surface area of the silicon-carbon composite material obtained in the above embodiment is 41.1 m 2 / g, pore volume is 0.17cm 3 / g, and the average pore size is 12.3nm. The thermogravimetric analysis results of the prepared silicon-carbon composite material show that the silicon content is 86.1wt%. According to the XPS analysis results, the nitrogen content is 1.02at%.
[0059] Example 4
[0060] This embodiment provides a method for preparing a silicon-carbon composite material, which specifically includes the following steps:
[0061] 1) 23.5 g of silicon powder (porous silicon, Hubei Benxing New Materials Co., Ltd.), 6.0 g of phenolic resin, 9.8 g of calcium chloride, 12.3 g of nano-magnesium oxide, 37.1 g of phosphoric acid solution (the concentration of the phosphoric acid solution is 85 wt%), and 15.6 g of thiourea were crushed and mixed, and ball-milled in a high-energy ball mill for 1 hour. The treated powder was placed in a boat, and the boat was placed in a tube furnace.
[0062] 2) In a nitrogen atmosphere, the nitrogen flow rate is 150 ml / min; the tubular furnace is heated to 800°C at a heating rate of 3°C / min and maintained for 5.0 hours, and then cooled to room temperature to obtain a silicon-carbon precursor; the silicon-carbon precursor powder is mixed with an HCl solution (the concentration of the HCl solution is 2M, and the amount added is 320 ml), stirred at 80°C for a total stirring time of 8 hours, and then washed with deionized water to a pH of 7.0, and then vacuum dried at 110°C for 24 hours to obtain the silicon-carbon composite material.
[0063] The specific surface area of the silicon-carbon composite material obtained in the above embodiment is 61.7 m 2 / g, pore volume is 0.20cm 3 / g, and the average pore size is 11.5nm. Thermogravimetric analysis results of the prepared silicon-carbon composite material show that the silicon content is 89.8wt%. According to the XPS analysis results, the nitrogen content is 1.33at%.
[0064] Example 5
[0065] This embodiment provides a method for preparing a silicon-carbon composite material, which specifically includes the following steps:
[0066] 1) 15.9 g of silicon powder (150 nm), 13.8 g of petroleum asphalt, 28.3 g of calcium chloride, 15.2 g of nano-calcium carbonate, 44.2 g of phosphoric acid solution (the concentration of the phosphoric acid solution is 85 wt%), and 8.5 g of ammonium hydrogen phosphate were ground and mixed, and ball-milled in a high-energy ball mill for 1 hour. The treated powder was placed in a boat, and the boat was placed in a tube furnace.
[0067] 2) In a nitrogen atmosphere, the nitrogen flow rate is 50 ml / min; the tube furnace is heated to 750°C at a heating rate of 1.5°C / min and maintained for 2.5 hours, and then cooled to room temperature to obtain a silicon-carbon precursor; the silicon-carbon precursor powder is mixed with an HCl solution (the concentration of the HCl solution is 2M, and the amount added is 180 ml), stirred at 80°C for a total stirring time of 8 hours, and then washed with deionized water to a pH of 7.0, and then vacuum dried at 110°C for 24 hours to obtain the silicon-carbon composite material.
[0068] The specific surface area of the silicon-carbon composite material obtained in the above embodiment is 53.8 m 2 / g, pore volume is 0.24cm 3 / g, and the average pore size is 13.1nm. The thermogravimetric analysis results of the prepared silicon-carbon composite material show that the silicon content is 87.9wt%. According to the XPS analysis results, the nitrogen content is 0.92at%.
[0069] Example 6
[0070] This embodiment provides a method for preparing a silicon-carbon composite material, which is different from Embodiment 1 in that only a single template agent, calcium chloride, is used. Specifically, the method includes the following steps:
[0071] 1) 25.0 g of silicon powder (150 nm), 5.0 g of coal hot-melt catalytic heavy components, 6.8 g of calcium chloride, 15.3 g of phosphoric acid solution (the concentration of the phosphoric acid solution is 85 wt%), and 6.0 g of thiourea are ground and mixed, and ball-milled in a high-energy ball mill for 1 hour. The treated powder is placed in a boat, and the boat is placed in a tube furnace.
[0072] 2) In a nitrogen atmosphere, the nitrogen flow rate is 150 ml / min; the tube furnace is heated to 850°C at a heating rate of 3°C / min and maintained for 2.5 hours, and then cooled to room temperature to obtain a silicon-carbon precursor; the silicon-carbon precursor powder is mixed with an HCl solution (the concentration of the HCl solution is 2M, and the amount added is 20 ml), stirred at 80°C for 8 hours, and then washed with deionized water to a pH of 7.0, and then vacuum dried at 110°C for 24 hours to obtain the silicon-carbon composite material.
[0073] The specific surface area of the silicon-carbon composite material obtained in the above embodiment is 50.3 m 2 / g, pore volume is 0.19cm 3 / g, and the average pore size is 11.8nm. Thermogravimetric analysis results of the prepared silicon-carbon composite material show that the silicon content is 85.3wt%. According to the XPS analysis results, the nitrogen content is 1.15at%.
[0074] Example 7
[0075] This embodiment provides a method for preparing a silicon-carbon composite material, which is different from Embodiment 3 in that potassium hydroxide or the like is used as a pore-forming agent instead of the phosphoric acid solution in Embodiment 3.
[0076] The specific surface area of the silicon-carbon composite material obtained in the above embodiment is 91.8 m 2 / g, pore volume is 0.2cm 3 / g, and the average pore size is 8.9nm. Thermogravimetric analysis results of the prepared silicon-carbon composite material show that the silicon content is 87wt%. According to the XPS analysis results, the nitrogen content is 1.18at%.
[0077] Example 8
[0078] This embodiment provides a method for preparing a silicon-carbon composite material, which differs from Embodiment 4 in that the heteroatom precursor is removed.
[0079] The specific surface area of the silicon-carbon composite material obtained in the above embodiment is 43.9 m 2 / g, pore volume is 0.18cm 3 / g, and the average pore size is 11.0nm. Thermogravimetric analysis results of the prepared silicon-carbon composite material show that the silicon content is 84.9wt%.
[0080] Example 9
[0081] This embodiment provides a method for preparing a silicon-carbon composite material, which is different from Embodiment 1 in that nano-magnesium oxide is used instead of calcium chloride.
[0082] The specific surface area of the silicon-carbon composite material obtained in the above embodiment is 40.9 m 2 / g, pore volume is 0.16cm 3 / g, and the average pore size is 14.3nm. Thermogravimetric analysis results of the prepared silicon-carbon composite material show that the silicon content is 83.9wt%. According to the XPS analysis results, the nitrogen content is 0.90at%.
[0083] Comparative Example 1
[0084] This comparative example provides a method for preparing a silicon-carbon composite material, which specifically comprises the following steps:
[0085] 1) 25.0 g of silicon powder (150 nm), 5.0 g of coal hot-melt catalytic heavy components, 15.3 g of phosphoric acid solution (the concentration of the phosphoric acid solution is 85 wt%), and 6.0 g of thiourea are ground and mixed, and ball-milled in a high-energy ball mill for 1 hour. The treated powder is placed in a boat, and the boat is placed in a tubular furnace.
[0086] 2) In a nitrogen atmosphere, the nitrogen flow rate is 150 ml / min; the tubular furnace is heated to 850°C at a heating rate of 3°C / min and maintained for 2.5 hours, and then cooled to room temperature to obtain a silicon-carbon precursor; the silicon-carbon precursor powder is mixed with an HCl solution (the concentration of the HCl solution is 2M, and the amount added is 20 ml), stirred at 80°C for a total stirring time of 8 hours, and then washed with deionized water to a pH of 7.0, and then vacuum dried at 110°C for 24 hours to obtain the silicon-carbon composite material.
[0087] The specific surface area of the silicon-carbon composite material obtained in the above comparative example is 23.1 m 2 / g, pore volume is 0.10cm 3 / g, and the average pore size is 22.3nm. Thermogravimetric analysis results of the prepared silicon-carbon composite material show that the silicon content is 83.7wt%. XPS analysis results show that the nitrogen content is 1.42at%.
[0088] Comparative Example 2
[0089] This comparative example provides a method for preparing a silicon-carbon composite material, which specifically comprises the following steps:
[0090] 1) 25.0 g of silicon powder (150 nm), 5.0 g of coal hot-dissolving catalytic heavy components, 5.0 g of nano zinc oxide, and 6.0 g of thiourea were ground and mixed, and ball-milled in a high-energy ball mill for 1 hour. The treated powder was placed in a boat, and the boat was placed in a tube furnace.
[0091] 2) In a nitrogen atmosphere, the nitrogen flow rate is 150 ml / min; the tubular furnace is heated to 850°C at a heating rate of 3°C / min and maintained for 2.5 hours, and then cooled to room temperature to obtain a silicon-carbon precursor; the silicon-carbon precursor powder is mixed with an HCl solution (the concentration of the HCl solution is 2M, and the amount added is 80 ml), stirred at 80°C for a total stirring time of 8 hours, and then washed with deionized water to a pH of 7.0, and then vacuum dried at 110°C for 24 hours to obtain the silicon-carbon composite material.
[0092] The specific surface area of the silicon-carbon composite material obtained in the above comparative example is 34.9 m 2 / g, pore volume is 0.13cm 3 / g, and the average pore size is 16.5nm. Thermogravimetric analysis results of the prepared silicon-carbon composite material show that the silicon content is 84.6wt%. According to XPS analysis results, the nitrogen content is 1.05at%.
[0093] Comparative Example 3
[0094] This comparative example provides a method for preparing a silicon-carbon composite material, which specifically comprises the following steps:
[0095] 1) 25.0 g of silicon powder (150 nm), 5.0 g of coal hot-melt catalytic heavy components, 6.8 g of calcium chloride, and 6.0 g of thiourea were ground and mixed, and ball-milled in a high-energy ball mill for 1 hour. The treated powder was placed in a boat, and the boat was placed in a tube furnace.
[0096] 2) In a nitrogen atmosphere, the nitrogen flow rate is 150 ml / min; the tubular furnace is heated to 850°C at a heating rate of 3°C / min and maintained for 2.5 hours, and then cooled to room temperature to obtain a silicon-carbon precursor; the silicon-carbon precursor powder is mixed with an HCl solution (the concentration of the HCl solution is 2M, and the amount added is 20 ml), stirred at 80°C for a total stirring time of 8 hours, and then washed with deionized water to a pH of 7.0, and then vacuum dried at 110°C for 24 hours to obtain the silicon-carbon composite material.
[0097] The specific surface area of the silicon-carbon composite material obtained in the above comparative example is 26.1 m 2 / g, pore volume is 0.15cm 3 / g, and the average pore size is 18.3nm. The thermogravimetric analysis results of the prepared silicon-carbon composite material show that the silicon content is 86.9wt%. According to the XPS analysis results, the nitrogen content is 1.14at%.
[0098] Comparative Example 4
[0099] This comparative example provides a method for preparing a silicon-carbon composite material, which specifically comprises the following steps:
[0100] 1) 25.0 g of silicon powder (150 nm), 5.0 g of coal hot-dissolving catalytic heavy components, and 6.0 g of thiourea were ground and mixed, and ball-milled in a high-energy ball mill for 1 hour. The treated powder was placed in a boat, and the boat was placed in a tube furnace.
[0101] 2) In a nitrogen atmosphere, the nitrogen flow rate is 150 ml / min; the tubular furnace is heated to 850°C at a heating rate of 3°C / min and maintained for 2.5 hours, and then cooled to room temperature to obtain a silicon-carbon precursor; the silicon-carbon precursor powder is mixed with an HCl solution (the concentration of the HCl solution is 2M, and the amount added is 20 ml), stirred at 80°C for a total stirring time of 8 hours, and then washed with deionized water to a pH of 7.0, and then vacuum dried at 110°C for 24 hours to obtain the silicon-carbon composite material.
[0102] The specific surface area of the silicon-carbon composite material obtained in the above comparative example is 19.7 m 2 / g, pore volume is 0.11cm 3 / g, pore size is 27.8nm. Thermogravimetric analysis results of the prepared silicon-carbon composite material show that the silicon content is 80.1wt%. XPS analysis results show that the nitrogen content is 1.30at%.
[0103] Test Example 1
[0104] This test example provides performance tests of the silicon-carbon composite materials of various embodiments and comparative examples, as follows:
[0105] (1) Test method for specific surface area, pore size distribution and pore volume of silicon-carbon composite materials: The test was carried out using a specific surface analyzer (JW-BK200C). The results are shown in Table 1. The samples were pretreated at 300°C for 10 h before testing.
[0106] (2) Method for detecting silicon content in silicon-carbon composite materials: A comprehensive thermal analyzer (Shanghai Yingnuo Precision Instrument Co., Ltd., model ZH-1450) was used. The detection conditions were heating at a rate of 10°C / min to 1000°C in air. The results are shown in Table 1.
[0107] (3) Morphology and composition of silicon-carbon composite materials: The morphology of the silicon-carbon composite materials was detected by high-resolution transmission electron microscopy (HRTEM, Philips, Netherlands, Tecnai G2F20). The morphology of the silicon-carbon composite material in Example 1 is shown in Figure 2The surface composition of the silicon-carbon composite material was obtained by X-ray photoelectron spectroscopy (XPS, Thermo K-Alphat, USA). The results of nitrogen content in the silicon-carbon composite materials of each embodiment and comparative example are shown in Table 1.
[0108] (4) Electrochemical properties of silicon-carbon composite materials:
[0109] Assemble button cells: Weigh silicon-carbon composite material, conductive agent super P, adhesive (adhesive includes 4227 (Guangzhou Rongdong New Materials Co., Ltd.) and CMC in a mass ratio of 1:1) in a mass ratio of 3:1:1, mix, add appropriate amount of deionized water, fully grind, and then apply it on the copper foil current collector. After vacuum drying at 120°C for 12 hours, the negative electrode plate is obtained. The negative electrode plate and the lithium sheet counter electrode are assembled into a button cell. The battery model is CR2032 button cell. The electrolyte is 1.16M LiPF6 solution. The solvent in the electrolyte includes EC, DMC and EMC in a volume ratio of 20:70:10. The electrolyte also includes 1wt% VC, 1wt% PS and 7wt% FEC. The separator used is Celgard polyethylene film.
[0110] Test method: On the LANHE CT3001A tester, the voltage range is 0.01-1.5V vs Li / Li+, the first cycle charge and discharge current density is 0.025C (105mA / g), and the subsequent cycle charge and discharge current density is 0.05C (210mA / g). The capacity retention rate and reversible specific capacity of the battery after 200 cycles are tested and analyzed.
[0111] Among them, the reversible specific capacity is obtained by testing the detection equipment, and the capacity retention rate is calculated as follows:
[0112] Capacity retention rate = specific capacity after 200 cycles / initial specific capacity × 100%
[0113] The test results of the above embodiments and comparative examples are shown in Table 1.
[0114] Table 1 Electrochemical properties of the silicon-carbon composite materials obtained in Examples 1-9 and Comparative Examples 1-4 when used as negative electrodes for lithium-ion batteries.
[0115]
[0116] As can be seen from Table 1, the silicon-carbon composite material prepared by the preparation method of the present invention in the embodiment has appropriate pore volume, pore diameter, and specific surface area. After being made into a battery, the first coulombic efficiency is greater than 88.9%, the capacity retention rate after 200 cycles is maintained at more than 89% of the initial discharge capacity, and the reversible specific capacity after 200 cycles is above 2000 mAh / g.
[0117] The main reason is that an appropriate pore-forming process is adopted, that is, the template agent and the pore-forming agent are combined to form an amorphous carbon layer with a unique pore structure coated on the outer layer of silicon. The carbon layer can not only buffer the expansion and contraction of silicon, but also act as a network for conducting electrons and ions, thereby adjusting the first effect, cycle stability, and reversible specific capacity of the silicon-carbon composite material after making a battery. By comparing Example 3 with Example 7, it can be concluded that phosphoric acid is better than potassium hydroxide as a pore-forming agent; by comparing Example 4 with Example 8, it can be concluded that nitrogen atom doping is beneficial to the electrochemical properties of the prepared silicon-carbon composite material. Compared with the examples, the specific surface area and pore volume of the silicon-carbon composite material obtained in Comparative Example 1 without the use of a template agent decreased, the pore size became larger, and the first effect, reversible specific capacity after 200 cycles, and capacity retention rate also decreased significantly. Comparative Examples 2-3 use a single template agent, and the specific surface area, pore volume, first effect, reversible specific capacity after 200 cycles, and capacity retention rate also decrease significantly, and the pore size becomes larger, indicating that a single template agent cannot achieve the technical effect of a composite template agent. Comparative Example 4 shows that not using the pore-forming process will further significantly reduce the specific surface area, pore volume, first effect, reversible specific capacity after 200 cycles, and capacity retention rate. As shown by the results of Comparative Examples 1-4, using a single pore-forming agent or template agent or not using the pore-forming process, a carbon layer with a corresponding pore structure cannot be formed, thereby affecting its coating on silicon, greatly reducing its first effect, cycle stability, and reversible specific capacity.
[0118] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.
Claims
1. A method for preparing a silicon-carbon composite material, characterized in that: The method comprises mixing a silicon source, a carbon source, a template agent and a pore forming agent, and sintering; Wherein, the template agent is at least one of nano magnesium oxide, nano zinc oxide, nano calcium carbonate, sodium chloride, potassium chloride and calcium chloride; The pore-forming agent is potassium hydroxide or phosphoric acid solution.
2. The preparation method according to claim 1, characterized in that: The template is at least two of nano magnesium oxide, nano zinc oxide, nano calcium carbonate, sodium chloride, potassium chloride and calcium chloride; and / or, The pore-forming agent is a phosphoric acid solution.
3. The preparation method according to claim 1, characterized in that: The template agent includes calcium chloride and nano zinc oxide; The concentration of the phosphoric acid solution is not less than 85 wt %.
4. The preparation method according to any one of claims 1 to 3, characterized in that The mass ratio of the template agent to the pore-forming agent is (3-60): (12-50).
5. The preparation method according to any one of claims 1 to 4, characterized in that: The mixing step also includes the step of adding a heteroatom precursor; Preferably, the heteroatom precursor is a nitrogen-containing compound; Preferably, the heteroatom precursor is at least one of melamine, ammonia, urea, thiourea and ammonium hydrogen phosphate; Preferably, the mass ratio of the heteroatom precursor to the template is (3-35):(3-60).
6. The preparation method according to any one of claims 1 to 5, characterized in that: The mass ratio of the silicon source, the carbon source and the template agent is (5-50): (2-40): (3-60); Preferably, the carbon source is at least one of petroleum asphalt, glucose, coal thermal catalytic heavy components, lignin, phenolic resin, epoxy resin and polyacrylonitrile; Preferably, the silicon source is at least one of nano-silicon, micro-silicon and porous silicon; Preferably, the particle size of the nano-silicon is 20-500nm; Preferably, the particle size of the micron silicon is 1-50 μm.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The specific steps of sintering include: heating to 350-1200°C at a heating rate of 0.5-20°C / min and then keeping the temperature for 0.1-20h; Preferably, the sintering is carried out under a protective atmosphere; Preferably, the protective atmosphere comprises at least one of an inert gas and nitrogen; Preferably, during the sintering, the flow rate of the protective atmosphere is 30-500 ml / min.
8. The preparation method according to any one of claims 1 to 7, characterized in that: The sintering step also includes a pickling step; Preferably, the pickling solution for pickling is at least one of hydrochloric acid, nitric acid and sulfuric acid; Preferably, the concentration of the pickling solution is 1-3 mol / L.
9. The silicon-carbon composite material obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the silicon-carbon composite material obtained by the preparation method according to any one of claims 1 to 8 in pole pieces and / or lithium-ion batteries.
Citation Information
Patent Citations
Silicon / carbon composite material for lithium ion battery and preparation method and application thereof
CN106450192A
Silicon-carbon composite material and preparation method thereof, negative pole piece, secondary battery and electric device
CN117174882A
Cited By
Low-expansion silicon-carbon material and preparation method thereof
CN120887424A