Preparation method of coal-based energy storage battery negative electrode material

By employing pulverization, shaping, and graphitization processes, combined with mechanical grinding and grading techniques, ash content is significantly reduced, resulting in the preparation of high-purity, high-performance lithium battery anode materials. This solves the problems of high cost, low purity, and poor cycle performance in existing technologies.

CN118908198AInactive Publication Date: 2024-11-08CHINA ENERGY GRP NINGXIA COAL IND CO LTD +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410953681.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for preparing lithium battery anode materials involve complex processes, high costs, low product purity, and poor cycle performance, failing to meet the quality requirements of energy storage batteries.

Method used

By employing pulverization, shaping, and graphitization processes, and through mechanical grinding and classification wheel grading, combined with ball milling shaping and high-temperature calcination, the ash content is significantly reduced, thus preparing high-purity anode materials.

Benefits of technology

Low-cost, high-efficiency physical ash removal was achieved, producing a negative electrode material with a purity of 99.9%, exhibiting excellent cycle performance and meeting the quality requirements of energy storage batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908198A_ABST
    Figure CN118908198A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a coal-based energy storage battery negative electrode material. The invention specifically provides a preparation method of a negative electrode material, which comprises the following steps: a pulverization step: providing raw coal particles, pulverizing the raw coal particles to obtain raw coal powder, and grading the raw coal powder to obtain a carbon powder precursor and a first grey matter component; a shaping step: performing ball-milling shaping on the carbon powder precursor, and grading the carbon powder precursor subjected to ball-milling shaping to obtain refined carbon powder and a second gray component; a graphitization step; and screening and demagnetizing. The preparation method is simple in process and low in cost, and the prepared negative electrode material is high in purity and excellent in energy storage performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of production of negative electrode materials for energy storage batteries, and in particular to a method for preparing negative electrode materials for energy storage batteries, and more particularly to a method for preparing low-cost coal-based negative electrode materials for energy storage batteries. Background Art

[0002] At present, lithium battery energy storage is in a period of rapid growth. The raw materials used for negative electrode materials for energy storage batteries are mainly low-sulfur petroleum coke. Due to the dual control of energy consumption, low-sulfur coke manufacturers have not seen significant expansion of production, and it is estimated that they will be in short supply in the future. The negative electrode manufacturing industry for energy storage batteries is also committed to finding substitutes for low-sulfur coke. Anthracite has a high carbon content, low sulfur content, and a dense internal structure, which can be used as a precursor for negative electrodes. However, it has a high ash content and low production and processing efficiency. It reacts with utensils and crucibles during high-temperature graphitization, which seriously affects the service life of utensils and crucibles. In addition, the graphite prepared by high-ash coal-based precursors has a high impurity content, which is obviously contrary to the requirements of high-safety, high-carbon, and low-cost negative electrode materials for energy storage.

[0003] Conventional ash removal methods include physical and chemical methods. Physical methods mainly include jigging, heavy medium and flotation. Under the premise of taking into account the cost, the current ash content of ash removal is about 3.5%. Chemical methods mainly include hydrofluoric acid method, conventional acid-base method, molten alkali leaching method and chemical coal method. Although these can greatly reduce the ash content, they are costly and polluting. While removing the ash, they will also change and destroy the original chemical structure of the coal, increase the number of holes on the surface of the precursor, and the graphite prepared by high-temperature graphitization has a large specific surface area and the pH does not meet the use requirements, which seriously affects the processing and cycle performance of coal-based materials at the battery end.

[0004] Patent publication number CN 116621154 A discloses a method for preparing a negative electrode material for a battery, and its electrode and battery. The method reports a method for preparing a negative electrode material for a battery from coal: the method first obtains coal particles less than 10 mm, mixes the coal particles, water and heavy medium, floats twice, then magnetically separates, and then treats with alkali and acid, and finally carbonizes, carbonizes and breaks up, and sieves to obtain a negative electrode material for a battery. This method uses flotation and alkali-acid method in the process of pre-treating raw coal to reduce ash content. The process is complex and costly. The advantage of low cost of coal raw materials has been weakened by flotation and alkali-acid method, and does not meet the requirements for low-cost preparation of negative electrode materials for energy storage.

[0005] Patent publication number CN 110745820 A discloses a method for purifying anthracite-based microcrystalline graphite for preparing negative electrode materials for lithium-ion batteries. The method mainly includes: anthracite-based microcrystalline graphite is subjected to two-stage jaw crushing, one-stage impact hammer crushing, and horizontal stirring mill-dry cyclone classification to prepare ultrafine powder with a particle size of less than 10μm, and two inhibitors, homemade emulsified kerosene collector and 2# oil foaming agent are used at the same time to perform one roughing and five fine cleaning to obtain a concentrate with a carbon content of not less than 90.0% as a flotation ore; in a constant temperature water bath, the flotation ore is placed in a mixed solution of one or more acids, stirred, ultrasonicated for 30-60 minutes, washed with water to pH=7, and then filtered and dried to obtain purified microcrystalline graphite. However, this method also uses an acid purification method, which is costly and polluting, and therefore its large-scale production application is limited.

[0006] Patent publication number CN 111146417 A discloses a fast-charge lithium-ion battery spherical graphite negative electrode material and its preparation method. First, anthracite is activated with KOH and graphitized at high temperature. The main function of KOH is to activate pores and remove silicon impurities in anthracite. Then it is mixed with a binder liquid phase for coating and spray-dried granulation to obtain a secondary particle structure. This method has a complex process. After KOH activation, a large amount of water washing is required, which causes water resource consumption, high cost and damage to the raw coal structure. The pH value and specific surface area of ​​the prepared material cannot be ensured. Although the rate performance is improved, the cycle performance of the material is deteriorated.

[0007] At present, the cost of raw materials for negative electrode materials has increased, so attention has been paid to anthracite, which has abundant reserves, low cost and great potential. When preparing negative electrode materials from anthracite, the existing technology mainly selects low-ash anthracite to prepare directly or first reduces the ash content of the raw coal before preparing the negative electrode material. Although the negative electrode material prepared directly from low-ash anthracite (ash content 3%-4%) removes most of the ash by high-temperature graphitization, the metal and non-metallic element impurity content of the material cannot be fully guaranteed when applied at the battery end, and during high-temperature graphitization, high ash impurities corrode the crucible, resulting in increased material processing costs. First, the ash content of the raw coal is reduced before preparing the negative electrode material. Physical and chemical methods are usually used for comprehensive ash removal, and then the negative electrode material is obtained through the preparation process of the negative electrode material. This method is costly and polluting, destroys the chemical structure of the raw coal, and although the prepared material has excellent rate performance, the pH value and specific surface area of ​​the material cannot be guaranteed, and it cannot be applied on a large scale in industrial applications. Summary of the invention

[0008] The purpose of the present invention is to provide a method for preparing anode materials of coal-based energy storage batteries, so as to solve the technical problems of the known preparation methods in the prior art, such as complex procedures, high costs, low product purity and poor cycle performance.

[0009] In order to achieve the above-mentioned object, according to one aspect of the present disclosure, a method for preparing a negative electrode material is provided, comprising the following steps: Step S1: pulverization: providing raw coal particles and pulverizing the raw coal particles to obtain raw coal powder, classifying the raw coal powder to obtain a carbon powder precursor and a first ash component, removing the first ash component, wherein the particle size D50 of the carbon powder precursor is 5-20 μm, the tap density is ≥0.48 g / cc, and the ash content is ≤3.0 wt%; Step S2: shaping: shaping the carbon powder precursor The ball-milled carbon powder precursor is graded to obtain refined carbon powder and a second ash component, and the second ash component is removed, wherein the particle size D50 of the refined carbon powder is 5-20 μm, the tap density is ≥0.66 g / cc, and the ash content is ≤2.5 wt%; step S3: graphitization: high-temperature calcining the refined carbon powder at a temperature of 2800°C or higher to obtain coal-based graphite; and step S4: screening and demagnetization: screening and demagnetizing the coal-based graphite to obtain a negative electrode material.

[0010] Furthermore, in step S1, the raw coal is preliminarily physically washed, the raw coal particle size is ≤10 mm, the vitrinite reflectance is ≥2.0 and the volatility is ≤10 wt%, and the ash content in the raw coal particles is ≤6 wt%, and the sulfur content is ≤0.5 wt%.

[0011] Furthermore, in step S1, the pulverization step is performed by one or more of mechanical milling, air flow milling and roller milling.

[0012] Further, in step S2, the shaping step is performed using one or more of a vertical shaping machine, a horizontal shaping machine and an intermittent shaping machine.

[0013] Further, in step S1, the raw coal powder is classified by a classifying wheel, and in step S2, the carbon powder precursor is classified by a classifying wheel.

[0014] Further, in step S1, the first ash component is discharged through the spiral discharge port, the rotation of the spiral discharge port is powered by a motor, and the motor is intermittently started by a frequency converter, the frequency converter controls the motor to start once every 1.5-5.0 minutes, and the running time of the motor each time it is turned on is 10 seconds.

[0015] Further, in step S2, the second gray component is discharged through the spiral discharge port. The rotation of the spiral discharge port is powered by a motor, and the motor is started intermittently through the control of a frequency converter. The frequency converter controls the motor to start once every 1.5-6.0 minutes, and the running time of the motor each time it is turned on is 10 seconds.

[0016] Furthermore, in step S3, the graphitization step is carried out in an Acheson crucible furnace or an inner tandem furnace, and the graphitization degree of the coal-based graphite is ≥90%.

[0017] Further, in step S4, screening is performed twice using a 270-325 mesh screen, and demagnetization is performed for 10-20 minutes using a 12000 Gauss demagnetization rod.

[0018] According to another aspect of the present disclosure, a negative electrode material is provided, which is prepared by any one of the above methods.

[0019] As mentioned above, the known method of using anthracite to prepare negative electrode materials for energy storage batteries has technical problems such as complex procedures, high cost, low product purity and poor cycle performance. According to the technical solution of the present disclosure, a method for preparing negative electrode materials for coal-based energy storage batteries is provided, wherein the raw material anthracite is subjected to preliminary coarse crushing to obtain raw coal particles, and then the raw coal particles are directly pulverized to a particle size D50 and a tap density within a specific range by mechanical grinding, so that the carbon powder precursor and the ash component in the pulverized raw coal powder are separated, and after classification by a classification wheel, a carbon powder precursor with a lower ash content and an ash component with a higher ash content are obtained, and the light carbon powder precursor rises due to the negative pressure of the air flow, while the ash component has a larger mass and sinks and aggregates. Then, the classified ash component is intermittently separated and discharged from the main machine cavity. Through mechanical grinding and classification, the ash component is separated and discharged from the spiral ash discharge port located at the upper side of the main grinding disc and the pulverizing chamber of the mechanical mill, thereby significantly reducing the ash content in the raw coal powder and realizing the primary physical ash removal of the raw coal powder.

[0020] Furthermore, by ball milling the separated carbon powder precursor, the edges and corners of the powder particles of the carbon powder precursor are removed, the sphericity is improved, the particle size D50 and the tap density of the carbon powder precursor are increased, and after classification by the classifying wheel, a refined carbon powder with a lower ash content and an ash component with a higher ash content are obtained. The light refined carbon powder rises due to the negative pressure of the airflow, while the ash component has a larger mass and sinks and aggregates. The classified ash component is then intermittently separated and discharged from the carbon powder precursor. Through ball milling and classification, the ash component can be further separated and discharged from the spiral ash discharge port located at the upper side of the main grinding disc and the crushing chamber of the shaper, thereby further significantly reducing the ash content in the carbon powder precursor and realizing the secondary physical ash removal of the raw coal powder. Anthracite powder with significantly reduced ash content is obtained through two-stage physical ash removal.

[0021] The present invention selects low-ash smokeless raw coal with abundant reserves and low cost, and integrates pulverization, shaping and ash removal through simple pulverization, shaping and graphitization process. The ash content can be significantly reduced only through the combination of pulverization and shaping process. The process is simple and the cost is low. The purpose of efficient physical ash removal is achieved without affecting the chemical structure of the raw coal. The purity of the prepared negative electrode material reaches 99.9% or higher, and the cycle performance is excellent, meeting the quality requirements of negative electrode materials for energy storage batteries. In addition, the graphitization degree of the negative electrode material prepared by graphitization treatment, screening and demagnetization of carbon powder reaches 90% or higher, and the specific surface area is ≤2.0m 2 / g, first discharge specific capacity ≥335mAh / g, Si element content ≤40ppm, pH is about 6.7, and the capacity retention rate is ≥99% after 50 charge and discharge cycles at room temperature and 1C. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0023] Figure 1 It is a schematic diagram of the core cavity structure of the mechanical grinding and shaping machine according to the present invention. DETAILED DESCRIPTION

[0024] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present disclosure will be described in detail below in conjunction with the embodiments.

[0025] In view of the deficiencies in the prior art mentioned in the background technology, a specific embodiment of the present disclosure provides a method for preparing a negative electrode material, characterized in that it includes the following steps: Step S1: pulverization: providing raw coal particles and pulverizing the raw coal particles to obtain raw coal powder, classifying the raw coal powder to obtain a carbon powder precursor and a first ash component, and removing the first ash component, wherein the particle size D50 of the carbon powder precursor is 5-20 μm, the tap density is ≥0.48 g / cc, and the ash content is ≤3.0 wt%; Step S2 : Shaping: ball-milling the carbon powder precursor, classifying the ball-milled carbon powder precursor to obtain refined carbon powder and a second ash component, removing the second ash component, wherein the particle size D50 of the refined carbon powder is 5-20μm, the tap density is ≥0.66g / cc, and the ash content is ≤2.5wt%; Step S3: Graphitization: high-temperature calcining the refined carbon powder at a temperature of 2800℃ or higher to obtain coal-based graphite; and Step S4: Screening and demagnetization: screening and demagnetizing the coal-based graphite to obtain the negative electrode material.

[0026] Raw coal particles (particle size of 20-50 mm) are obtained by preliminarily coarsely crushing the raw anthracite (e.g., anthracite with an ash content in the range of 3.0 wt%-6 wt%), and then the raw coal particles are directly pulverized to a particle size D50 and a tap density within a specific range (e.g., the particle size D50 of the carbon powder precursor is 5-20 μm, and the tap density is ≥ 0.48 g / cc) through a mechanical mill, so that the carbon powder precursor and the ash component in the pulverized raw coal powder are separated, and after classification by a classifying wheel, a carbon powder precursor with a lower ash content and an ash component with a higher ash content are obtained. Due to the different densities of the carbon powder precursor and the ash component, the light carbon powder precursor rises to the top discharge port of the device through the negative pressure of the air flow, while the ash component has a larger mass and sinks and aggregates. Then, the classified ash component is separated and discharged from the raw coal powder under the intermittent opening of the variable frequency motor. Through mechanical grinding and grading, the ash components are separated and discharged from the spiral ash discharge port located at the upper side of the main grinding disc and the crushing chamber of the mechanical mill, thereby significantly reducing the ash content in the raw coal powder and realizing primary physical ash removal of the raw coal powder.

[0027] Furthermore, by ball milling the separated carbon powder precursor, the edges and corners of the powder particles of the carbon powder precursor are removed, the sphericity is improved, the particle size D50 and the tap density of the carbon powder precursor are increased, and after classification by the classifying wheel, a refined carbon powder with a lower ash content and an ash component with a higher ash content are obtained. Due to the different densities of the refined carbon powder and the ash component, the light refined carbon powder rises to the discharge port through the negative pressure of the air flow, while the ash component has a larger mass and sinks and aggregates. In this way, the classified ash component is intermittently separated and discharged from the carbon powder precursor. Through ball milling and classification, the ash component can be further separated and discharged from the spiral ash discharge port located at the upper side of the main grinding disc and the crushing chamber of the shaping machine, thereby further significantly reducing the ash content in the carbon powder precursor and realizing the secondary physical ash removal of the raw coal powder. Anthracite powder with significantly reduced ash content is obtained by two-stage physical ash removal through pulverization and shaping processes. Subsequently, the refined carbon powder with reduced ash content is subjected to high-temperature graphitization treatment and screening and demagnetization to obtain the negative electrode material for energy storage batteries of the present invention, which has favorable capacity and capacity retention performance and can meet the quality requirements for negative electrode materials for energy storage batteries.

[0028] Preferably, the particle size D50 of the carbon powder precursor is 6-19 μm. For example, the particle size D50 of the carbon powder precursor is 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, etc. Preferably, the tap density of the carbon powder precursor is ≥ 0.48 g / cc. For example, the tap density of the carbon powder precursor is 0.48 g / cc, 0.49 g / cc, 0.5 g / cc, 0.51 g / cc, 0.52 g / cc, 0.53 g / cc, 0.54 g / cc, 0.55 g / cc, 0.56 g / cc, 0.57 g / cc, 0.58 g / cc, 0.59 g / cc, 0.60 g / cc, 0.61 g / cc, 0.62 g / cc, 0.63 g / cc, 0.64 g / cc, 0.65 g / cc, 0.66 g / cc, 0.67 g / cc, 0.68 g / cc, etc. The particle size D50 and tap density of the carbon powder precursor are within the scope of the present disclosure, which can further improve the classification of the carbon powder precursor and the ash component in the raw coal powder, improve the separation efficiency, and thus further reduce the ash component in the raw coal powder.

[0029] Preferably, the particle size D50 of the refined carbon powder is 6-19 μm. For example, the particle size D50 of the refined carbon powder is 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, etc. Preferably, the tap density of the refined carbon powder is ≥ 0.66 g / cc. For example, the tap density of the refined carbon powder is 0.66 g / cc, 0.67 g / cc, 0.68 g / cc, 0.69 g / cc, 0.70 g / cc, 0.71 g / cc, 0.72 g / cc, 0.73 g / cc, 0.74 g / cc, 0.75 g / cc, 0.76 g / cc, 0.77 g / cc, 0.78 g / cc, 0.79 g / cc, 0.80 g / cc, 0.82 g / cc, 0.84 g / cc, 0.86 g / cc, 0.90 g / cc, etc. The particle size D50 and tap density of the refined carbon powder are within the scope of the present disclosure, which can further improve the classification of the refined carbon powder and the ash component in the carbon powder precursor, improve the separation efficiency, and thus further reduce the ash component in the carbon powder precursor.

[0030] Preferably, in the pulverization step, the raw coal is physically washed in advance, the raw coal particle size is ≤10mm, the vitrinite reflectance is ≥2.0 and the volatility is ≤10wt%, and the ash content in the raw coal particles is ≤6wt%, and the sulfur content is ≤0.5wt%. For example, the particle size of the raw coal powder is 10mm, 9mm, 8mm, 7mm, 6mm, etc., the vitrinite reflectance is 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, etc., the volatility is 10wt%, 9wt%, 8wt%, 7wt%, 6wt%, 5wt%, 4wt%, 3wt%, etc., and the ash content in the raw coal particles is 6wt%, 5.9wt%, 5.8wt%, 5.7wt%, 5.6wt%, 5.5wt%, 5.4wt%. %, 5.3wt%, 5.2wt%, 5.1wt%, 5.0wt%, 4.9wt%, 4.8wt%, 4.7wt%, 4.6wt%, 3.9wt%, 3.8wt%, 3.7wt%, 3.6wt%, 3.5wt%, 3.4wt%, 3.3wt%, 3.2wt%, 3.1wt%, 3wt%, etc., and the sulfur content is 0.5wt%, 0.4wt%, 0.3wt%, 0.2wt%, 0.1wt%, etc. The parameters of the raw coal powder and the raw coal particles in the pulverization step are within the above ranges, which can help to further reduce the process cost and help to further reduce the ash content in the carbon powder precursor and the refined carbon powder, so as to obtain a negative electrode material for energy storage batteries with higher purity and better energy storage effect.

[0031] Preferably, the pulverizing step is performed by one or more of a mechanical mill, a jet mill and a roller mill. More preferably, the pulverizing step is performed by a mechanical mill.

[0032] Preferably, the shaping step is performed using one or more of a vertical shaping machine, a horizontal shaping machine and an intermittent shaping machine. More preferably, the shaping step is performed using a vertical shaping machine.

[0033] Preferably, a classifying wheel is used to classify the raw coal powder in the pulverizing step, and a classifying wheel is used to classify the carbon powder precursor in the shaping step. Using a classifying wheel to classify the raw coal powder and the carbon powder precursor respectively can improve the separation efficiency between the carbon powder and the ash component, further reduce the ash content in the raw coal powder and the carbon powder precursor, and improve the purity and energy storage performance of the negative electrode material product.

[0034] Preferably, in the pulverizing step, the first ash component is discharged through the spiral discharge port, the rotation of the spiral discharge port is powered by a motor, and the motor is intermittently started by a frequency converter, the frequency converter controls the motor to start once every 1.5-5.0 minutes, and the motor runs for 10 seconds each time it is turned on. More preferably, in the pulverizing step, the frequency converter controls the motor to start once every 1.5 minutes, 2.0 minutes, 2.5 minutes, 3.0 minutes, 3.5 minutes, 4.0 minutes, 4.5 minutes, 5.0 minutes, etc.

[0035] Preferably, in the shaping step, the second gray component is discharged through the spiral discharge port, the rotation of the spiral discharge port is powered by a motor, and the motor is intermittently started by a frequency converter, the frequency converter controls the motor to start once every 1.5-6.0 minutes, and the motor runs for 10 seconds each time it is turned on. More preferably, in the shaping step, the frequency converter controls the motor to start once every 1.5 minutes, 2.0 minutes, 2.5 minutes, 3.0 minutes, 3.5 minutes, 4.0 minutes, 4.5 minutes, 5.0 minutes, 5.5 minutes, 6.0 minutes, etc.

[0036] In the pulverizing and shaping steps, the frequency converter controls the start-up frequency and running time of the motor within the scope of the present disclosure, which can be conducive to realizing intermittent start-up of the motor, thereby intermittently discharging the ash components from the main machine cavity through the spiral ash discharge port located at the upper side of the main grinding disc and the pulverizing cavity of the mechanical mill and the shaping machine, respectively. This can further save costs, improve the removal efficiency of the ash components, and further reduce the ash content in the raw coal powder and the carbon powder precursor.

[0037] Preferably, in the graphitization step, the graphitization step is carried out in an Acheson crucible furnace or an inner tandem furnace, and the graphitization degree of the coal-based graphite is ≥90%.

[0038] Preferably, in the screening and demagnetization step, the screening is performed twice using a 270-325 mesh screen, and the demagnetization is performed for 10-20 minutes using a 12000 gauss demagnetization rod. The screening and demagnetization parameters are within the scope of the present disclosure, which can help reduce the impurity content in the negative electrode material and improve the product quality, thereby further improving the capacity and capacity retention characteristics of the energy storage battery containing the negative electrode material.

[0039] Another specific embodiment of the present disclosure provides a negative electrode material prepared by the method of the present invention.

[0040] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0041] Example 1

[0042] (1) Pulverization: Provide anthracite raw material (i.e., raw coal), and perform preliminary washing of the anthracite raw material (but do not perform chemical acid-base ash removal). The particle size of the anthracite raw material is 20-50 mm, the ash content is 5.8 wt%, the S content is ≤0.5 wt%, and the C content is 92 wt%. The anthracite raw material is crushed by a 10 mm jaw crusher to obtain anthracite raw coal particles with a particle size of ≤10 mm. The coarsely crushed anthracite raw coal particles are crushed by a mechanical mill and classified by a grading wheel to obtain a carbon powder precursor and a first ash component. A carbon powder discharge port is provided at the top of the mechanical mill, and a spiral ash discharge port is provided at the upper side of the main grinding disc and the crushing chamber of the mechanical mill. The spiral ash discharge port is powered by a motor controlled by a frequency converter. The frequency converter controls the motor to start once every 1.5 minutes. The motor runs for 10 seconds each time it is turned on, and the first ash component in the device is removed by intermittent startup. The carbon powder precursor is discharged from the carbon powder outlet at the top of the device. The particle size D50 of the carbon powder precursor is 8.5 μm, the tap density is 0.5 g / cc, and the ash content is 2.2 wt %.

[0043] (2) Shaping: Use a vertical shaping machine to perform ball milling shaping on the carbon powder precursor obtained in step (1), that is, the shape of the carbon powder precursor particles is adjusted by ball milling, and a grading wheel is used for grading to obtain refined carbon powder and the second ash component. The vertical shaping machine is provided with a carbon powder discharge port at the top, and a spiral ash discharge port is provided at the upper side of the main grinding disc and the crushing chamber of the vertical shaping machine. The spiral ash discharge port is powered by a motor controlled by a frequency converter. The frequency converter controls the motor to start once every 3 minutes. The motor runs for 10 seconds each time it is turned on, and the second ash component in the device is removed by intermittent startup. The refined carbon powder is discharged from the carbon powder discharge port at the top of the device. The particle size D50 of the refined carbon powder is 8.9μm, the tap density is 0.68g / cc, and the ash content is 1.5wt%.

[0044] (3) Graphitization: The refined carbon powder obtained in step (2) is calcined at a high temperature in an Acheson crucible furnace, with the graphitization temperature being about 2800° C., to obtain coal-based graphite.

[0045] (4) Screening and demagnetization: The coal-based graphite obtained in step (3) is screened twice, the first screening using a 325-mesh screen and the second screening using a 270-mesh screen, and then the coal-based graphite passing through the 270-mesh screen is demagnetized using a 12,000 gauss demagnetization rod for 10 minutes to obtain a negative electrode material for an energy storage battery.

[0046] Example 2

[0047] The negative electrode material was prepared in the same manner as in Example 1, except that in step (1), the frequency converter controlled the motor to be turned on once every 3 minutes, the tap density of the carbon powder precursor was 0.48 g / cc, and the ash content was 2.5 wt%; in step (2), the frequency converter controlled the motor to be turned on once every 6 minutes, the tap density of the refined carbon powder was 0.66 g / cc, and the ash content was 2.1 wt%.

[0048] Example 3

[0049] The negative electrode material was prepared in the same manner as in Example 1, except that in step (1), the tap density of the carbon powder precursor was 0.50 g / cc and the ash content was 2.0 wt%; in step (2), the inverter controlled the motor to be turned on once every 1.5 minutes, and the tap density of the refined carbon powder was 0.67 g / cc and the ash content was 1.5 wt%.

[0050] Example 4

[0051] The negative electrode material is prepared in the same manner as in Example 1, except that the particle size D50 of the carbon powder precursor in step (1) is 14.1 μm, the tap density is 0.55 g / cc, and the ash content is 2.3 wt%; and the particle size D50 of the refined carbon powder in step (2) is 15.2 μm, the tap density is 0.70 g / cc, and the ash content is 1.8 wt%.

[0052] Example 5

[0053] The negative electrode material is prepared in the same manner as in Example 1, except that in step (1), the frequency converter controls the motor to be turned on once every 3 minutes, the particle size D50 of the carbon powder precursor is 14.1 μm, the tap density is 0.55 g / cc, and the ash content is 2.6 wt%; in step (2), the frequency converter controls the motor to be turned on once every 6 minutes, the particle size D50 of the refined carbon powder is 15.2 μm, the tap density is 0.72 g / cc, and the ash content is 2.2 wt%.

[0054] Example 6

[0055] The negative electrode material is prepared in the same manner as in Example 1, except that in step (1), the frequency converter controls the motor to be turned on once every 3 minutes, the particle size D50 of the carbon powder precursor is 18.5 μm, the tap density is 0.62 g / cc, and the ash content is 2.7 wt%; and in step (2), the particle size D50 of the refined carbon powder is 19.6 μm, the tap density is 0.75 g / cc, and the ash content is 2.5 wt%.

[0056] Example 7

[0057] The negative electrode material is prepared in the same manner as in Example 1, except that in step (1), the frequency converter controls the motor to be turned on once every 5 minutes, the particle size D50 of the carbon powder precursor is 18.5 μm, the tap density is 0.62 g / cc, and the ash content is 2.75 wt%; in step (2), the frequency converter controls the motor to be turned on once every 5 minutes, the particle size D50 of the refined carbon powder is 19.6 μm, the tap density is 0.76 g / cc, and the ash content is 2.5 wt%.

[0058] Comparative Example 1

[0059] (1) Pulverization: Provide anthracite raw material (i.e., raw coal), perform preliminary washing of the anthracite raw material (but do not perform chemical acid-base ash removal), the particle size of the anthracite raw material is 20-50 mm, the ash content is 5.8 wt%, the S content is ≤0.5 wt%, and the C content is 92 wt%. The anthracite raw material is crushed by a 10 mm jaw crusher to obtain anthracite raw coal particles with a particle size of ≤10 mm, the coarsely crushed anthracite raw coal particles are crushed by a mechanical mill, and a carbon powder precursor is obtained after crushing, the particle size D50 of the carbon powder precursor is 8.5 μm, the tap density is 0.5 g / cc, and the ash content is 5.8 wt%.

[0060] (2) The carbon powder precursor obtained in step (1) is subjected to ball milling and shaping treatment using a vertical shaping machine, i.e., the shape of the carbon powder precursor particles is adjusted by ball milling, and refined carbon powder is obtained after ball milling and shaping. The refined carbon powder has a particle size D50 of 8.9 μm, a tap density of 0.61 g / cc, and an ash content of 5.7 wt%.

[0061] (3) Graphitization: The refined carbon powder obtained in step (2) is calcined at a high temperature in an Acheson crucible furnace, with the graphitization temperature being about 2800° C., to obtain coal-based graphite.

[0062] (4) Screening and demagnetization: The coal-based graphite obtained in step (3) is screened twice, the first screening using a 325-mesh screen and the second screening using a 270-mesh screen, and then the coal-based graphite passing through the 270-mesh screen is demagnetized using a 12,000 gauss demagnetization rod for 10 minutes to obtain a negative electrode material for an energy storage battery.

[0063] Comparative Example 2

[0064] The negative electrode material is prepared in the same manner as in Comparative Example 1, except that the ash content of the anthracite raw material in step (1) is 7.3 wt%, the particle size D50 of the carbon powder precursor is 14.1 μm, the tap density is 0.57 g / cc, and the ash content is 7.3 wt%; and the particle size D50 of the refined carbon powder in step (2) is 15.2 μm, the tap density is 0.63 g / cc, and the ash content is 7.3 wt%.

[0065] Comparative Example 3

[0066] (1) Pulverization: A low-sulfur petroleum coke raw material is provided, wherein the ash content is 0.8 wt%, the S content is ≤0.5%, and the C content is 90 wt%. The petroleum coke raw material is crushed by a 10 mm jaw crusher to obtain petroleum coke particles with a particle size of ≤10 mm. The crushed petroleum coke particles are crushed by a mechanical mill to obtain a carbon powder precursor. The carbon powder precursor has a particle size D50 of 18.5 μm, a tap density of 0.55 g / cc, and an ash content of 0.8 wt%.

[0067] (2) The carbon powder precursor obtained in step (1) is subjected to ball milling and shaping treatment using a vertical shaping machine, i.e., the shape of the carbon powder precursor particles is adjusted by ball milling, and refined carbon powder is obtained after ball milling and shaping. The refined carbon powder has a particle size D50 of 19.6 μm, a tap density of 0.62 g / cc, and an ash content of 0.8 wt%.

[0068] (3) Graphitization: The refined carbon powder obtained in step (2) is calcined at a high temperature in an Acheson crucible furnace, with the graphitization temperature being about 2800° C., to obtain coal-based graphite.

[0069] (4) Screening and demagnetization: The coal-based graphite obtained in step (3) is screened twice, the first screening using a 325-mesh screen and the second screening using a 270-mesh screen, and then the coal-based graphite passing through the 270-mesh screen is demagnetized using a 12,000 gauss demagnetization rod for 10 minutes to obtain a negative electrode material for an energy storage battery.

[0070] Performance Testing

[0071] Determination of specific surface area

[0072] The specific surface area was determined according to the method specified in GB / T 19587. The test equipment used was Besed 3H-2000A.

[0073] Determination of first discharge specific capacity

[0074] The first discharge specific capacity was determined according to the method in the national standard GB / T 24533-2019 for "graphite negative electrode materials for lithium-ion batteries". The test equipment used was the CT2001 battery tester.

[0075] Determination of trace element Si

[0076] The digestion of graphite adopts the super microwave digestion method, the solvent uses a mixture of hydrochloric acid and perchloric acid, the temperature is raised to 260 degrees, and the temperature is kept for 40 minutes to ensure that the graphite is completely digested. The trace element Si content test equipment uses an inductively coupled plasma atomic emission spectrometer ICP-OES.

[0077] Determination of battery capacity retention after 50 cycles

[0078] The capacity retention rate was determined according to the method in the national standard GB / T 24533-2019 for "graphite negative electrode materials for lithium-ion batteries". The test was carried out at room temperature, the program was set to cycle 50 times, and the capacity retention rate was calculated as follows: the first lithium desorption capacity was recorded as the initial value, and the ratio of the lithium desorption capacity after N cycles to the initial value was recorded as the capacity retention rate after N cycles.

[0079] The performance test results of the above embodiments and comparative examples are shown in Table 1 below.

[0080] Table 1

[0081]

[0082]

[0083] From the above results, it can be seen that according to the embodiments 1-7 of the method for preparing the negative electrode material of the present invention, the negative electrode material is obtained by combining pulverization (making powder) and shaping, and then graphitizing and screening to remove magnetism. The specific surface area of ​​the negative electrode material of the present invention is ≤2.0m 2 / g, Si element content ≤40ppm, the first discharge specific capacity of the energy storage battery using the material is greater than 335mAh / g, and the capacity retention rate after 50 charge and discharge cycles is ≥98%. In contrast, the specific surface area, Si element content, first discharge specific capacity, and capacity retention rate after 50 charge and discharge cycles of the negative electrode materials prepared in Comparative Examples 1-3, whose preparation processes are not within the scope of the present application, are significantly inferior to those of the negative electrode materials prepared by the process method of the present invention.

[0084] The above embodiments are merely descriptions of the technical solutions of the present disclosure, rather than limiting the scope thereof. Although ordinary technicians in the field can make various modifications with reference to the above examples, they should be within the protection scope of the present disclosure as long as they do not deviate from the design spirit of the present disclosure.

[0085] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those described herein, for example.

[0086] The above description only relates to specific embodiments of the present disclosure and is not intended to limit the present disclosure. For those skilled in the art, the present disclosure may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present disclosure shall be included in the protection scope of the present disclosure.

Claims

1. A method for preparing a negative electrode material, characterized in that: The steps include: Step S1: pulverization: providing raw coal particles and pulverizing the raw coal particles to obtain raw coal powder, classifying the raw coal powder to obtain a carbon powder precursor and a first ash component, removing the first ash component, wherein the carbon powder precursor has a particle size D50 of 5-20 μm, a tap density of ≥0.48 g / cc, and an ash content of ≤3.0 wt%; Step S2: shaping: ball-milling the carbon powder precursor, classifying the ball-milled carbon powder precursor to obtain refined carbon powder and a second ash component, removing the second ash component, wherein the refined carbon powder has a particle size D50 of 5-20 μm, a tap density of ≥0.66 g / cc, and an ash content of ≤2.5 wt%; Step S3: graphitization: calcining the refined carbon powder at a temperature of 2800° C. or higher to obtain coal-based graphite; as well as Step S4: Screening and demagnetization: Screening and demagnetizing the coal-based graphite to obtain the negative electrode material.

2. The method according to claim 1, characterized in that In the step S1, the raw coal is physically washed in advance, the raw coal particle size is ≤10 mm, the vitrinite reflectance is ≥2.0 and the volatility is ≤10 wt%, and the ash content in the raw coal particles is ≤6 wt%, and the sulfur content is ≤0.5 wt%.

3. The method according to claim 1 or 2, characterized in that: In the step S1, the pulverization step is performed by one or more of mechanical milling, air flow milling and roller milling.

4. The method according to claim 1 or 2, characterized in that: In step S2, the shaping step is performed using one or more of a vertical shaping machine, a horizontal shaping machine and an intermittent shaping machine.

5. The method according to claim 1 or 2, characterized in that: In the step S1, the raw coal powder is classified by a classifying wheel, and in the step S2, the carbon powder precursor is classified by a classifying wheel.

6. The method according to claim 1 or 2, characterized in that: In the step S1, the first ash component is discharged through a spiral discharge port, the rotation of the spiral discharge port is powered by a motor, and the motor is intermittently started by a frequency converter, the frequency converter controls the motor to start once every 1.5-5.0 minutes, and the running time of the motor each time it is turned on is 10 seconds.

7. The method according to claim 1 or 2, characterized in that: In the step S2, the second ash component is discharged through a spiral discharge port. The rotation of the spiral discharge port is powered by a motor, and the motor is intermittently started by a frequency converter. The frequency converter controls the motor to start once every 1.5-6.0 minutes, and the running time of the motor is 10 seconds each time it is turned on.

8. The method according to claim 1 or 2, characterized in that: In step S3, the graphitization step is performed in an Acheson crucible furnace or an inner tandem furnace, and the graphitization degree of the coal-based graphite is ≥90%.

9. The method according to claim 1 or 2, characterized in that: In the step S4, the screening is performed twice using a 270-325 mesh screen, and the demagnetization is performed for 10-20 minutes using a 12000 Gauss demagnetization rod.

10. A negative electrode material, characterized in that: The negative electrode material is prepared by the method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for purifying anthracite-based microcrystalline graphite for preparing lithium ion battery negative electrode material

    CN110745820A

  • Fast-charging type lithium ion battery spherical graphite anode material and a preparation method thereof

    CN111146417A

  • Preparation method of battery negative electrode material and electrode and battery thereof

    CN116621154A

  • Coking coal quality improving device and quality improving method

    CN106378250A

  • Coal crushing, grading and sorting device and method

    CN106391268A