Method for preparing silicon carbide by adding reinforced waste graphite and silicon waste into biomass ash
By mixing silicon waste and waste graphite with biomass ash for vacuum calcination, high-purity silicon carbide is prepared, which solves the problems of resource waste and environmental pollution, reduces production costs and energy consumption, and achieves sustainable utilization of resources.
Patent Information
- Application Number
- CN202411281371.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-13
AI Technical Summary
The existing technology fails to effectively use biomass ash and waste graphite to prepare high-quality silicon carbide, resulting in resource waste and environmental pollution problems. The production cost of traditional silicon carbide is high and energy consumption is high.
By mixing silicon waste and waste graphite powder with biomass ash in a certain proportion, vacuum calcining at high temperature, high-purity silicon carbide is prepared, and the quality and yield of silicon carbide are improved by using the catalytic action of biomass ash.
The reuse of waste resources has been achieved, the production cost of silicon carbide has been reduced, environmental pollution has been reduced, resource utilization efficiency has been improved, and energy consumption and greenhouse gas emissions have been reduced.
Smart Images

Figure CN118908216A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing silicon carbide by adding biomass ash to reinforce waste graphite and silicon waste, and belongs to the technical field of secondary resource utilization. Background Art
[0002] With the rapid development of science and technology, graphite and silicon are widely used in many fields such as electronics, semiconductors, and new energy. However, a large amount of waste graphite and silicon waste is generated during production and use. The accumulation of these wastes not only occupies a large amount of land resources, but also may pollute the soil, water and air, bringing great pressure to the environment. At the same time, as important resources, the reserves of graphite and silicon are not inexhaustible, and the effective utilization of waste resources has become an inevitable requirement for sustainable development.
[0003] Silicon carbide is an important material with excellent properties. It has the characteristics of high hardness, high melting point, high thermal conductivity, high chemical stability, etc. It is widely used in abrasives, refractory materials, semiconductor devices, high-temperature structural materials and other fields. With the development of various industries, the demand for silicon carbide continues to grow. Traditional silicon carbide production methods often rely on high-purity carbon and silicon sources, which are costly and energy-intensive.
[0004] Using waste graphite and silicon waste as the main raw materials and strengthening them with biomass ash to produce high-quality silicon carbide not only provides a new way to reuse waste resources, but also reduces the production cost of silicon carbide and improves resource utilization efficiency. It has important practical significance and broad application prospects.
[0005] At present, there are two related patents on the preparation of silicon carbide using waste graphite and silicon waste: a method for preparing high-quality silicon carbide from diamond wire cutting waste (CN107651690A); a method for preparing high-quality silicon carbide from crystalline silicon cutting waste (CN107651691A). The above patents all prepare high-quality silicon carbide by cutting waste. The current existing technology does not involve the preparation of silicon carbide using biomass and waste graphite.
[0006] In patent 2024111964714, an attempt was made to prepare high-purity silicon by combining biomass with alkali metal carbonates or hydroxides. In later research and exploration, a technology for preparing relatively high-purity silicon carbide was developed, leading to the present invention. Summary of the invention
[0007] The present invention is aimed at the fact that there is no record of using biomass ash to strengthen silicon waste and waste graphite to prepare high-quality silicon carbide in the prior art. On the one hand, the present invention solves the problem of silicon waste and waste graphite polluting the environment and avoids waste of resources. On the other hand, it utilizes the strengthening effect of biomass such as coffee shells to turn waste into treasure and bring great economic benefits.
[0008] A method for preparing silicon carbide by adding biomass ash to reinforce waste graphite and silicon waste, the specific steps are as follows:
[0009] (1) crushing, grinding and sieving waste silicon and waste graphite respectively to obtain powders, thereby obtaining waste silicon powder and waste graphite powder, wherein the obtained powder has a particle size distribution of 50 to 150 μm;
[0010] (2) drying and crushing the selected biomass to obtain biomass powder;
[0011] (3) placing the biomass powder into a corundum crucible, roasting and keeping the mixture warm in an oxygen-containing atmosphere, and cooling the mixture after the heat preservation to obtain biomass ash;
[0012] (4) Grinding and mixing biomass ash with silicon waste powder and waste graphite powder in a certain proportion to obtain a mixture, placing the mixture into a high-purity graphite crucible and placing it in a muffle furnace, evacuating the furnace, and setting a temperature program to react the mixture at a high temperature; the mixture is composed of A and biomass ash, wherein A is composed of silicon waste powder and waste graphite powder in a mass ratio of 65-70:30-35; the content of biomass ash in the mixture is 1-10%; the vacuum roasting temperature is 1410-1700°C,
[0013] (5) After the reaction is completed, the product is cooled to room temperature to obtain a high-purity silicon carbide product.
[0014] The present invention discloses a method for preparing silicon carbide by adding biomass ash to reinforce waste graphite and silicon waste. In step (1), the silicon waste and waste graphite are sieved to achieve a particle size distribution of 50 to 150 μm.
[0015] The present invention provides a method for preparing silicon carbide by adding biomass ash to reinforce waste graphite and silicon waste. In step (2), the biomass is selected from at least one of coffee husks, tobacco straws, cotton straws, rice straws, wheat straws, corn straws, soybean straws and rice husks, preferably at least one of coffee husks, rice husks, rice straws and tobacco straws, and more preferably coffee husks and tobacco straws.
[0016] The present invention provides a method for preparing silicon carbide by adding biomass ash to reinforced waste graphite and silicon waste. In step (3), the roasting temperature is 600-1000°C and the holding time is 60-180 minutes. The reason why the present invention controls the holding time to 60-180 minutes is to ensure that the biomass is completely roasted and only ash remains. If the holding time is too short, it will lead to problems such as the biomass charcoal not being completely burned out. In the actual production process, the heating rate can be controlled at 5-15°C / min, such as 10°C / min, 12°C / min, etc.
[0017] The present invention provides a method for preparing silicon carbide by adding biomass ash to reinforce waste graphite and silicon waste. In step (4), the silicon waste content in mixture A is 65-70wt.%, the waste graphite content is 30-35wt.%, and the biomass ash content in the mixture is 1-10wt.%, preferably 1-2.5%, and more preferably 1-2%.
[0018] The present invention provides a method for preparing silicon carbide by adding biomass ash to reinforced waste graphite and silicon waste, wherein in step (4), the vacuum degree of vacuum roasting is 10 -3 ~50Pa, vacuum roasting temperature is 1410~1700℃, and holding time is 60~240min. In actual production process, heating rate can be controlled at 5-20℃ / min, such as 10℃ / min, 12℃ / min, 15℃ / min, etc.
[0019] Preferably, tobacco straw is roasted in an air atmosphere and then added to the mixture so that the biomass ash content is 1 to 1.1%.
[0020] The present invention provides a method for preparing silicon carbide by adding biomass ash to reinforced waste graphite and silicon waste, wherein the purity of the silicon carbide obtained in step (5) is ≥95.3%. After optimization, the purity of the silicon carbide is greater than 98%.
[0021] At present, carbothermal reduction has become a promising method due to its economy, high efficiency and large-scale preparation. In the carbothermal reduction process, the raw materials (carbon source and silicon source) have an important influence on the formation of SiC. At present, petroleum coke (or coal coke) is mainly used as a raw material to produce SiC in industry. Using waste graphite instead of graphite as a carbon source for preparing SiC and using microsilica waste generated by industrial production instead of silicon source can reduce the cost of preparing SiC. In addition, some alkali metals in biomass ash, such as K and Na elements, can delay the graphitization of the carbon source and promote the formation of SiC.
[0022] The beneficial effects of the present invention are:
[0023] The use of biomass ash to strengthen waste graphite and silicon waste to prepare silicon carbide has the following beneficial effects:
[0024] 1. Reusing waste graphite and silicon waste avoids the waste of these resources and reduces the dependence on primary resources; it conforms to the concept of circular economy, helps to achieve sustainable utilization of resources and reduces pressure on the environment;
[0025] 2. Biomass ash is originally a waste. By using it to prepare silicon carbide, the resource utilization of biomass ash is realized. By adding biomass ash to strengthen and / or catalyze the reaction process, the quality of silicon carbide is improved. Compared with the traditional preparation method, the use of waste graphite and silicon waste can reduce the cost of raw materials;
[0026] 3. It reduces the pollution of waste graphite, silicon waste and biomass ash to the environment and reduces the pressure of waste disposal; it may have lower energy consumption and less greenhouse gas emissions during the preparation process, which is more environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is the SEM image of the silicon carbide product in Example 1.
[0028] Figure 2 This is the SEM image of the silicon carbide product in Comparative Example 1. DETAILED DESCRIPTION
[0029] The present invention is further described in detail below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited to the described contents.
[0030] The mass percentage of Si in the silicon waste powder used in the examples and comparative examples of the present invention is 75-88%;
[0031] The mass percentage of C in the waste graphite powder used in the embodiments and comparative examples of the present invention is 70-85%. In the embodiments and comparative examples of the present invention, most impurities will float up to form slag during the smelting process; therefore, in laboratory operation, after cooling, the upper surface impurities (the upper surface is the direction of the crucible opening) can be directly cut off or polished off to obtain a silicon carbide product with higher purity. When used in industry, slag removal can be used to remove impurities.
[0032] Embodiment 1:
[0033] A method for preparing silicon carbide by adding biomass ash to reinforce waste graphite and silicon waste, the specific steps are as follows:
[0034] (1) crushing, grinding and sieving the silicon waste and waste graphite respectively to obtain silicon waste powder and waste graphite powder, wherein the particle size of the silicon waste powder is 75 μm and the particle size of the waste graphite powder is 75 μm;
[0035] (2) processing the tobacco straw to remove unprocessed tobacco leaves, and then drying and crushing the tobacco straw to obtain tobacco straw powder;
[0036] (3) putting tobacco straw powder into a corundum crucible, placing it in a muffle furnace, heating it to 600° C. at a heating rate of 10° C. / min, keeping it warm for 120 min in air, and cooling it in the furnace after the end of the keeping warm to obtain tobacco straw ash;
[0037] (4) taking 1wt.% tobacco straw ash and 99wt.% A, mixing them evenly and loading them into a high-purity graphite crucible, placing them in a muffle furnace, evacuating the furnace to a pressure of 10Pa, heating the furnace at a rate of 10°C / min to 1500°C, and performing vacuum roasting for 120min; the A is composed of 70wt.% silicon waste powder and 30wt.% waste graphite powder;
[0038] (5) After the heat preservation is completed, the product is cooled to room temperature, and impurities on the surface are removed to obtain a high-purity silicon carbide product.
[0039] The purity of silicon carbide obtained in this embodiment is 98.91%.
[0040] Example 1-1
[0041] The other conditions were the same as those in Example 1, except that: the tobacco straw powder was replaced with an equal mass of coffee husk powder;
[0042] The purity of silicon carbide obtained in this embodiment is 98.31%.
[0043] Example 1-2
[0044] Other conditions were the same as those in Example 1, except that an equal mass of rice husk powder was used to replace tobacco straw powder; and the purity of silicon carbide obtained in this example was 95.47%.
[0045] Examples 1-3
[0046] The other conditions were the same as those in Example 1, except that: the tobacco straw powder was replaced with an equal mass of cotton straw powder;
[0047] The purity of silicon carbide obtained in this embodiment is 96.40%.
[0048] Examples 1-4
[0049] The other conditions were the same as those in Example 1, except that: the tobacco straw powder was replaced by rice straw powder of equal mass;
[0050] The purity of silicon carbide obtained in this embodiment is 96.77%.
[0051] Examples 1-5
[0052] The other conditions were the same as those in Example 1, except that: the tobacco straw powder was replaced with wheat straw powder of equal mass;
[0053] The purity of silicon carbide obtained in this embodiment is 97.83%.
[0054] Examples 1-6
[0055] Other conditions were the same as those in Example 1, except that: an equal mass of corn stalk powder was used to replace tobacco stalk powder;
[0056] The purity of silicon carbide obtained in this embodiment is 95.14%.
[0057] Examples 1-7
[0058] The other conditions were the same as those in Example 1, except that: the tobacco straw powder was replaced with an equal mass of soybean straw powder;
[0059] The purity of silicon carbide obtained in this embodiment is 97.33%.
[0060] Embodiment 2:
[0061] A method for preparing silicon carbide by adding biomass ash to reinforce waste graphite and silicon waste, the specific steps are as follows:
[0062] (1) crushing, grinding and sieving silicon waste and waste graphite to obtain silicon waste powder and waste graphite powder, wherein the particle size of the silicon waste powder is 50 μm and the particle size of the waste graphite powder is 50 μm;
[0063] (2) drying and crushing the coffee husks to obtain coffee husk powder;
[0064] (3) The coffee shell powder is placed in a corundum crucible, placed in a muffle furnace, and heated to 700° C. at a heating rate of 10° C. / min. The temperature is kept at this temperature for 120 min in air. After the temperature is kept at this temperature, the coffee shell ash is obtained by cooling the crucible in the furnace.
[0065] (4) Take 2wt.% coffee husk ash and 98wt.% A, mix them evenly and put them into a high-purity graphite crucible, place it in a muffle furnace, and evacuate the furnace until the vacuum degree is 10 -3 Pa, heating to 1450°C at 10°C / min and performing vacuum roasting for 180min; the A is composed of 69wt.% silicon waste powder and 31wt.% waste graphite powder;
[0066] (5) After the heat preservation is completed, the product is cooled to room temperature, and impurities on the surface are removed to obtain a high-purity silicon carbide product.
[0067] The purity of silicon carbide obtained in this embodiment is 98.1%.
[0068] Example 3
[0069] A method for preparing silicon carbide by adding biomass ash to reinforce waste graphite and silicon waste, the specific steps are as follows:
[0070] (1) crushing, grinding and sieving silicon waste and waste graphite to obtain silicon waste powder and waste graphite powder, wherein the particle size of the silicon waste powder is 100 μm and the particle size of the waste graphite powder is 100 μm;
[0071] (2) drying and crushing the rice husk to obtain rice husk powder;
[0072] (3) The rice husk powder is placed in a corundum crucible, placed in a muffle furnace, and heated to 800° C. at a heating rate of 10° C. / min. The temperature is kept at this temperature for 90 minutes under air conditions. After the temperature is kept at this temperature, the rice husk ash is obtained by cooling the crucible in the furnace.
[0073] (4) 3 wt.% rice husk ash and 97 wt.% A were mixed and uniformly loaded into a high-purity graphite crucible, placed in a muffle furnace, evacuated to a vacuum degree of 20 Pa, and heated to 1550° C. at a rate of 10° C. / min for vacuum roasting for 150 min; the A was composed of 68 wt.% silicon waste powder and 32 wt.% waste graphite powder;
[0074] (5) After the heat preservation is completed, the product is cooled to room temperature, and impurities on the surface are removed to obtain a high-purity silicon carbide product.
[0075] The purity of silicon carbide obtained in this embodiment is 96.37%.
[0076] Example 4
[0077] A method for preparing silicon carbide by adding biomass ash to reinforce waste graphite and silicon waste, the specific steps are as follows:
[0078] (1) crushing, grinding and sieving silicon waste and waste graphite to obtain silicon waste powder and waste graphite powder, wherein the particle size of the silicon waste powder is 125 μm and the particle size of the waste graphite powder is 125 μm;
[0079] (2) drying and crushing the cotton stalks to obtain cotton stalk powder;
[0080] (3) The cotton straw powder is placed in a corundum crucible, placed in a muffle furnace, and heated to 900° C. at a heating rate of 10° C. / min. The temperature is kept at this temperature for 120 min under air conditions. After the temperature is kept at this temperature, the cotton straw ash is obtained by cooling the crucible in the furnace.
[0081] (4) Take 4wt.% cotton straw ash and 96wt.% A, mix them evenly and put them into a high-purity graphite crucible, place it in a muffle furnace, and evacuate the furnace until the vacuum degree is 10 -3 Pa, heating to 1600°C at 10°C / min and performing vacuum roasting for 180min; the A is composed of 67wt.% silicon waste powder and 33wt.% waste graphite powder,
[0082] (5) After the heat preservation is completed, the product is cooled to room temperature to obtain a high-purity silicon carbide product.
[0083] The purity of silicon carbide obtained in this embodiment is 96.95%.
[0084] Example 5
[0085] A method for preparing silicon carbide by adding biomass ash to reinforce waste graphite and silicon waste, the specific steps are as follows:
[0086] (1) crushing, grinding and sieving silicon waste and waste graphite to obtain silicon waste powder and waste graphite powder, wherein the particle size of the silicon waste powder is 150 μm and the particle size of the waste graphite powder is 150 μm;
[0087] (2) drying and crushing the corn stalks to obtain corn stalk powder;
[0088] (3) The corn straw powder was placed in a corundum crucible, placed in a muffle furnace, and heated to 1000°C at a heating rate of 10°C / min, and kept warm for 60 minutes under air conditions. After the end of the heat preservation, the crucible was cooled in the furnace to obtain coffee shell ash;
[0089] (4) 4 wt.% coffee husk ash and 96 wt.% A were mixed and uniformly loaded into a high-purity graphite crucible, placed in a muffle furnace, evacuated to a vacuum degree of 50 Pa, and heated to 1500° C. at a rate of 10° C. / min for vacuum roasting for 240 min; the A was composed of 66 wt.% silicon waste powder and 34 wt.% waste graphite powder;
[0090] (5) After the heat preservation is completed, the product is cooled to room temperature to obtain a high-purity silicon carbide product.
[0091] The purity of silicon carbide obtained in this embodiment is 97.59%.
[0092] Comparative Example 1:
[0093] A method for preparing silicon carbide by adding biomass ash to reinforce waste graphite and silicon waste, the specific steps are as follows:
[0094] (1) crushing, grinding and sieving silicon waste and waste graphite to obtain silicon waste powder and waste graphite powder, wherein the particle size of the silicon waste powder is 75 μm and the particle size of the waste graphite powder is 75 μm;
[0095] (2) 70 wt.% of silicon waste powder and 30 wt.% of waste graphite powder were mixed and uniformly loaded into a high-purity graphite crucible, placed in a muffle furnace, evacuated to a vacuum degree of 10 Pa, and heated to 1500° C. at a rate of 10° C. / min for vacuum roasting for 120 min;
[0096] (3) After the heat preservation is completed, the product is cooled to room temperature to obtain a high-purity silicon carbide product.
[0097] The purity of silicon carbide obtained in this comparative example is 93.78%, and obvious Si impurities exist in the product.
[0098] Comparative Example 2
[0099] A method for preparing silicon carbide by adding biomass ash to reinforce waste graphite and silicon waste, the specific steps are as follows:
[0100] (1) crushing, grinding and sieving silicon waste and waste graphite to obtain silicon waste powder and waste graphite powder, wherein the particle size of the silicon waste powder is 50 μm and the particle size of the waste graphite powder is 50 μm;
[0101] (2) 69 wt.% of silicon waste powder and 31 wt.% of waste graphite powder were mixed and evenly loaded into a high-purity graphite crucible, placed in a muffle furnace, and evacuated to a vacuum degree of 10 -3 Pa, heating at 10°C / min to 1450°C and calcining in vacuum for 180min;
[0102] (3) After the heat preservation is completed, the product is cooled to room temperature to obtain a high-purity silicon carbide product.
[0103] The purity of silicon carbide obtained in this comparative example is 91.84%.
[0104] Comparative Example 3
[0105] A method for preparing silicon carbide by adding biomass ash to reinforce waste graphite and silicon waste, the specific steps are as follows:
[0106] (1) crushing, grinding and sieving silicon waste and waste graphite to obtain silicon waste powder and waste graphite powder, wherein the particle size of the silicon waste powder is 100 μm and the particle size of the waste graphite powder is 100 μm;
[0107] (2) 67 wt.% of silicon waste powder and 33 wt.% of waste graphite powder were mixed and uniformly loaded into a high-purity graphite crucible, placed in a muffle furnace, evacuated to a vacuum degree of 20 Pa, and heated to 1550° C. at a rate of 10° C. / min for vacuum roasting for 150 min;
[0108] (3) After the heat preservation is completed, the product is cooled to room temperature to obtain a high-purity silicon carbide product.
[0109] The purity of silicon carbide obtained in this comparative example is 89.27%.
[0110] The specific embodiments of the present invention are described in detail above, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A method for preparing silicon carbide by adding biomass ash to reinforce waste graphite and silicon waste, characterized in that: The steps include: (1) crushing, grinding and sieving waste silicon and waste graphite respectively to obtain waste silicon powder and waste graphite powder, wherein the obtained powder has a particle size distribution of 50 to 150 μm; (2) drying and crushing the selected biomass to obtain biomass powder; (3) placing the biomass powder into a corundum crucible, roasting and keeping the mixture warm in an oxygen-containing atmosphere, and cooling the mixture after the heat preservation to obtain biomass ash; (4) Grinding and mixing biomass ash with silicon waste powder and waste graphite powder in a certain proportion to obtain a mixture, placing the mixture into a high-purity graphite crucible and placing it in a muffle furnace, evacuating the furnace, and reacting the mixture at a high temperature; the mixture is composed of A and biomass ash, wherein A is composed of silicon waste powder and waste graphite powder in a mass ratio of 65-70:30-35; the content of biomass ash in the mixture is 1-10%; the vacuum roasting temperature is 1410-1700°C, (5) After the reaction is completed, the product is cooled to room temperature to obtain a high-purity silicon carbide product.
2. The method for preparing silicon carbide by adding waste graphite and silicon waste to biomass ash according to claim 1, characterized in that: In step (2), the biomass is selected from at least one of coffee husks, tobacco straws, cotton straws, rice straws, wheat straws, corn straws, soybean straws and rice husks.
3. The method for preparing silicon carbide by adding waste graphite and silicon waste to biomass ash according to claim 2, characterized in that: In step (2), the biomass is selected from at least one of coffee husks, rice husks, rice straws and tobacco straws, and more preferably at least one of coffee husks and tobacco straws.
4. The method for preparing silicon carbide by adding waste graphite and silicon waste to biomass ash according to claim 1, characterized in that: In step (3), the calcination temperature is 600-1000° C., and the insulation time is 60-180 min.
5. The method for preparing silicon carbide by adding waste graphite and silicon waste to biomass ash according to claim 1, characterized in that: In step (4), the silicon waste content in the mixture A is 65-70wt.%, the waste graphite content is 30-35wt.%, and the biomass ash content in the mixture is 1-2.5%, and more preferably 1-2%.
6. The method for preparing silicon carbide by adding waste graphite and silicon waste to biomass ash according to claim 5, characterized in that: After tobacco straw is roasted in air atmosphere, the biomass ash is added into the mixture so that the content of the biomass ash is 1 to 1.1%.
7. The method for preparing silicon carbide by adding waste graphite and silicon waste to biomass ash according to claim 1, characterized in that: In step (4), the vacuum degree of vacuum roasting is 10 -3 ~50Pa, the vacuum calcination temperature is 1410~1700℃, and the holding time is 60~240min.
8. The method for preparing silicon carbide by adding waste graphite and silicon waste to biomass ash according to claim 1, characterized in that: The purity of the silicon carbide obtained in step (5) is ≥95.3%.
9. The method for preparing silicon carbide by adding waste graphite and silicon waste to biomass ash according to claim 1, characterized in that: The purity of the silicon carbide obtained in step (5) is greater than 98%.
Citation Information
Patent Citations
Method for synthesizing beta-SiC nano-wire
CN101306816A
Method for preparing silicon carbide nano line
CN101386409A
Method for preparing silicon carbide powder from polycrystalline silicon cutting wastes
CN105293498A
Silicon carbide nano-powder and preparation method thereof
CN118343762A
MANUFACTURING METHOD OF HIGH PURITY SiC
JP2019119629A
Cited By
Regeneration and recovery method of silicon carbide in silicon melt refining slag
CN119858921A