Biomass-based silicon-carbon negative electrode material and preparation method thereof

Through activation of biomass-based porous carbon material and nano-silicon deposition, combined with phenolic resin coating, the problem of volume change and poor cycle stability of silicon material in lithium-ion batteries is solved, and silicon with low cost, high specific capacity and excellent cycle performance is achieved Carbon anode material.

CN118908219AActive Publication Date: 2024-11-08HEFEI GUOXUAN HIGH TECH POWER ENERGY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410959250.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

The volume of silicon materials in existing lithium-ion batteries changes greatly during the lithium-ion deliquification process, resulting in poor powdering and falling off and cycle stability. The high-temperature synthesis of porous carbon materials is high cost and is not conducive to battery performance.

Method used

The biomass-based porous carbon material is activated by selective oxidation treatment, combined with silane deposition to form nanosilicon, followed by coating with phenolic resin to improve conductivity and stability.

Benefits of technology

The low cost, high specific capacity and excellent cycle stability of silicon carbon negative electrode materials are achieved, and the discharge capacity can reach 1400mAh/g~1600mAh/g, which significantly improves the first-time efficiency and cycle performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908219A_ABST
    Figure CN118908219A_ABST
Patent Text Reader

Abstract

The invention discloses a biomass-based silicon-carbon negative electrode material and a preparation method thereof.The preparation method comprises the steps that S1, porous biomass charcoal powder is placed in a reaction furnace, silicon source gas and inert gas are introduced, high-temperature calcination is conducted for 2-8 h at the temperature of 450-700 DEG C, and silicon-carbon powder is obtained; and S2, mixing the silicon-carbon powder with a phenolic resin precursor solution, heating, stirring and polymerizing, then carrying out solid-liquid separation, and sintering the obtained solid substance at 600-800 DEG C in an inert atmosphere for 4-6 hours to obtain the silicon-carbon composite material. The silicon-carbon negative electrode material disclosed by the invention takes biomass as a raw material, is low in cost, and has excellent specific capacity and cycling stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion battery materials, and in particular to a biomass-based silicon-carbon negative electrode material and a preparation method thereof. Background Art

[0002] At present, with the popularity of electric vehicles, the demand for high energy density lithium-ion batteries is growing. Silicon materials are expected to have a high theoretical capacity (>4000mAh / g) and a low lithium insertion potential (<0.4V). During the process of lithium insertion and de-lithiation, the silicon material will undergo a volume change of more than 400%, causing the silicon material to pulverize and fall off, forming a large amount of SEI film, so the cycle stability of the silicon negative electrode is poor. Compared with crystalline silicon, the amorphous silicon obtained by silane deposition has a smaller volume change and is more conducive to the electrochemical performance. However, most of the carbon matrices for silane deposition on the market are porous carbon materials prepared from organic polymers. The porous carbon obtained in this way is complicated to prepare and has a high cost, which is not conducive to the widespread application of silicon-carbon materials. Moreover, the current silicon-carbon materials generally adopt high-temperature synthesis methods, resulting in larger silicon grains, which is not conducive to the cycle performance of the battery. Summary of the invention

[0003] Based on the technical problems existing in the background technology, the present invention proposes a biomass-based silicon-carbon negative electrode material and a preparation method thereof.

[0004] The present invention provides a method for preparing a biomass-based silicon-carbon negative electrode material, comprising the following steps:

[0005] S1. Place the porous biomass carbon powder in a reaction furnace, introduce silicon source gas under an inert atmosphere, and calcine at a high temperature of 450° C. to 700° C. for 2 to 8 hours to obtain silicon carbon powder;

[0006] The preparation method of the porous biomass carbon powder comprises: heating a biomass raw material in an oxidant solution under acidic conditions to obtain a biomass precursor; mixing the biomass precursor with an activator and ball milling, and then calcining at a high temperature of 700° C. to 900° C. for 1 to 8 hours in an inert atmosphere to obtain the porous biomass carbon powder;

[0007] S2, mixing the silicon-carbon powder and the phenolic resin precursor solution, heating and stirring to polymerize, and then separating the solid and the liquid, and sintering the obtained solid material at a high temperature of 600° C. to 800° C. for 4 to 6 hours under an inert atmosphere to obtain the obtained solid material.

[0008] In the preparation method of the biomass-based silicon-carbon negative electrode material proposed in the present invention, the biomass is first boiled in an oxidizing solution under acidic conditions to selectively remove the lignin and hemicellulose components in the biomass raw material. This process increases the specific surface area of ​​the raw material and makes the skeleton of the biomass itself clearer, which is conducive to further activation and subsequent establishment of the carbon skeleton.

[0009] Subsequently, an alkali or salt activator is used to carbonize and activate the raw material. During this step, the alkali / salt reacts with the carbon matrix to form pores and produce a large amount of gas, which is conducive to the increase of pores. At the same time, metal ions enter the carbon matrix, which expands the interlayer spacing of the carbon crystals, which is conducive to the entry of the activator and the reaction. After calcination, washing and drying, a porous carbon matrix with a large specific surface area and abundant pores is obtained. The biomass carbon material treated by this method has an increased specific surface area and an increase in surface functional groups, which is conducive to the infiltration of the activator and further etching of the carbon material, making the pore-forming process more fully and uniformly reacting, and obtaining a porous carbon with a larger pore volume, a narrower pore size range, and a more uniform pore distribution. This type of porous carbon is easy for silane gas to enter the pores and decompose during the deposition process, obtaining a material in which nano-silicon is evenly distributed in the carbon matrix, which is conducive to alleviating the volume expansion of the material during the charge and discharge process;

[0010] Afterwards, a silicon source gas is used to decompose and deposit a large amount of nano-silicon on the porous carbon matrix. Due to the rich specific surface area and pore size confinement of the porous carbon, it is equivalent to putting these nano-silicon in cages, which limits the growth of nano-silicon crystals, thereby forming nano-silicon with smaller grains, and obtaining a silicon-carbon material in which the nano-silicon is confined and evenly distributed between the porous carbon skeletons;

[0011] Finally, phenolic resin is used to carbon-coat the silicon-carbon material to modify the porous surface, reduce the specific surface area, improve the electrical conductivity, protect the internal nanostructure, reduce contact with the electrolyte, and at the same time improve the processing performance and enhance the slurry stability of the material.

[0012] Preferably, in the method for preparing the porous biomass carbon powder, the preparation step of the biomass precursor is: heating the oxidant solution to a certain temperature, then adding the biomass raw material, then dripping acetic acid, and continuing the heating treatment to obtain the biomass precursor.

[0013] Preferably, the oxidant solution is heated to 60-100°C.

[0014] Preferably, the volume of the acetic acid added dropwise is 1% to 3% of the volume of the oxidant solution.

[0015] Preferably, in the method for preparing the porous biomass carbon powder, the mass ratio of the biomass raw material to the oxidant is 200-500:100-500; the concentration of the oxidant solution is 10-200 g / L. By controlling the amount and concentration of the oxidant during the selective oxidation pretreatment of the biomass in the method for preparing the porous biomass carbon powder, it is beneficial to fully activate the carbon skeleton and further improve the uniformity of the porous carbon pore size, thereby more effectively improving the cycle performance of the silicon-carbon material.

[0016] Preferably, the biomass raw material is at least one of coconut shells, peanut shells, wheat straw, rice husks, rice straw, reed leaves, and corn leaves.

[0017] Preferably, the oxidant is at least one of hydrogen peroxide, perchloric acid, sodium chlorate and sodium hypochlorite.

[0018] Preferably, the solvent of the oxidant solution is water.

[0019] Preferably, in the method for preparing the porous biomass carbon powder, the temperature of the heating treatment under acidic conditions is 60 to 100°C and the time is 8 to 12 hours. By controlling the conditions for the selective oxidation pretreatment of biomass in the method for preparing the porous biomass carbon powder, it is beneficial to fully activate the carbon skeleton and further improve the uniformity of the porous carbon pore size, thereby more effectively improving the cycle performance of the silicon-carbon material.

[0020] In the preparation of the biomass precursor, after the heating treatment, conventional subsequent processing steps such as cooling, washing and drying are also included.

[0021] Preferably, in the method for preparing the porous biomass carbon powder, the mass ratio of the biomass precursor to the activator is 1:1 to 1:6. By controlling the mass ratio of the biomass precursor to the activator, the degree of reaction between the carbon skeleton and the activator can be controlled to obtain porous carbon with different specific surface areas and pore volumes, thereby affecting the amount of silicon deposition, thereby achieving the purpose of regulating the capacity and first coulombic efficiency of the silicon-carbon material.

[0022] Preferably, the activator is at least one of potassium hydroxide, sodium hydroxide, sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, and zinc chloride.

[0023] In the preparation method of porous biomass carbon powder, after high-temperature calcination, conventional subsequent treatment steps such as acid washing, water washing, and drying are also included.

[0024] Preferably, in S1, the silicon source gas is at least one of silicon tetrafluoride, silicon tetrachloride, trichlorosilane, dichlorosilane and disilane.

[0025] In the present invention, the inert atmosphere refers to an atmosphere formed by an inert gas, and the inert gas refers to a non-reactive gas that does not participate in the reaction, preferably nitrogen, argon or a combination thereof.

[0026] Preferably, in S2, the conditions for heating and stirring polymerization are: stirring polymerization at 60° C. to 100° C. for 8 to 12 hours. By controlling the reaction conditions for heating and stirring polymerization in S2, a denser and more complete carbon-silicon material surface coating layer can be obtained, further improving the electrical conductivity and cycle stability of the material.

[0027] Preferably, the phenolic resin precursor solution is obtained by dissolving phenols and aldehydes in a mixed solvent of an acid aqueous solution and ethanol; the phenols are at least one of phenol, resorcinol, m-cresol and xylenol; the aldehydes are at least one of formaldehyde, acetaldehyde, propionaldehyde and butyraldehyde; the molar ratio of the phenols to the aldehydes is 1:2 to 2:1; the volume ratio of the acid aqueous solution to ethanol is 1:3 to 3:1; the acid aqueous solution is an aqueous solution of at least one of hydrochloric acid, oxalic acid, phosphoric acid and sulfuric acid, and the concentration is 0.5 mol / L to 3 mol / L.

[0028] Preferably, the specific surface area of ​​the porous biomass carbon powder is 1000 cm 2 / g~3500cm 2 / g. Controlling the specific surface area of ​​the porous biomass carbon powder within a suitable range, the volume space it provides is more suitable for the deposition of nano-silicon and fully provides the volume expansion space required by silicon in the charge and discharge cycle, which is conducive to further improving the cycle performance of the material.

[0029] A biomass-based silicon-carbon negative electrode material is prepared by the preparation method.

[0030] Preferably, in the biomass-based silicon-carbon negative electrode material, the mass of silicon accounts for 30% to 60% of the total mass of the material. By controlling the silicon content in the biomass-based silicon-carbon negative electrode material, that is, the silicon-carbon ratio, silicon-carbon materials suitable for different specific surface areas and pore volumes can be obtained, thereby achieving the purpose of adjusting and controlling the capacity and first coulombic efficiency of the silicon-carbon material.

[0031] The beneficial effects of the present invention are as follows:

[0032] The present invention uses biomass carbon as porous carbon raw material, which is activated after selective oxidation treatment to obtain a carbon material with rich pore size. The specific surface area of ​​the carbon material can reach 1000cm 2 / g~3500cm 2 / g, and then through silane deposition to form nano-silicon is confined between the porous carbon skeleton uniformly distributed silicon-carbon material, and finally through the coating of the phenolic resin carbonization to obtain the silicon-carbon negative electrode. The silicon-carbon negative electrode material obtained by this method has a low cost, the silicon in the material is evenly distributed in the carbon matrix, and no silicon crystals are formed, and it has excellent specific capacity and cycle stability. Its capacity can reach 1400mAh / g to 1600mAh / g at 0.8V. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is an SEM image of the biomass-based silicon-carbon negative electrode material prepared in Example 2 of the present invention.

[0034] Figure 2 This is the XRD image of the biomass-based silicon-carbon negative electrode material prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0035] The technical solution of the present invention is described in detail below through specific embodiments.

[0036] Example 1

[0037] Preparation of biomass-based silicon-carbon anode materials:

[0038] S1. Place the porous biomass carbon powder in a rotary kiln, introduce argon gas for replacement for 1 hour, then heat to 600°C at a heating rate of 2°C / min, introduce disilane and keep warm for 6 hours, and obtain silicon-carbon powder after cooling;

[0039] The preparation method of the porous biomass carbon powder is as follows: 500 g of sodium hypochlorite is dissolved in 3 L of water, heated to 100 ° C, 500 g of wheat straw is added, and then 50 mL of acetic acid is dripped into it and continued to heat at 100 ° C for 12 hours, and then washed and dried after cooling to obtain a biomass precursor; potassium hydroxide and potassium carbonate are mixed in a mass ratio of 1:1 to obtain an activator, 1500 g of the activator is mixed with 300 g of the biomass precursor and ground for 10 hours, and then transferred to an argon atmosphere and calcined at 900 ° C for 8 hours, and then washed with hydrochloric acid, washed with water, and dried to obtain a specific surface area of ​​3000 cm 2 / g~3300cm 2 / g porous biochar powder;

[0040] S2, after mixing the silicon-carbon powder with the phenolic resin precursor solution, stirring and polymerizing at 80°C for 12 hours, collecting the precipitate, transferring it to a tubular furnace and calcining it at 800°C under argon conditions for 4 hours to obtain a biomass-based silicon-carbon negative electrode material;

[0041] The phenolic resin precursor solution is obtained by dissolving phenol and formaldehyde in a mixed solvent at a molar ratio of 6:7, and the mixed solvent is composed of a 1M hydrochloric acid aqueous solution and ethanol at a volume ratio of 1:1.

[0042] In the biomass-based silicon-carbon negative electrode material obtained above, the mass of silicon accounts for 60% of the total mass of the material.

[0043] The obtained biomass-based silicon-carbon negative electrode material and metal lithium were used to form a half-cell for electrochemical performance testing, with a test rate of 0.1C (first time) + 0.5C (cycle) and a charge and discharge voltage of 0.005-0.8V. The results showed that the discharge capacity of the negative electrode sheet can reach 1750.2mAh / g, with a first efficiency of 83.0%.

[0044] The obtained biomass-based silicon-carbon negative electrode material was evenly mixed with graphite in a mass ratio of 5:95 as a composite negative electrode material. NCM622 was used as the positive electrode, and the processes of slurry mixing, coating, rolling, slitting, die cutting, lamination, welding of pole ears, top and side sealing, baking, and liquid injection were carried out to assemble 7Ah soft-pack batteries. After fractionation, a room temperature cycle test was carried out at a current density of 1C / 1C. The first efficiency of the battery cell was 85.5%. After 600 cycles of the full battery, the capacity retention rate was 87.3%.

[0045] Example 2

[0046] Preparation of biomass-based silicon-carbon anode materials:

[0047] S1. Place the porous biomass carbon powder in a rotary kiln, introduce argon gas for replacement for 1 hour, then heat to 550°C at a heating rate of 5°C / min, introduce monosilane and keep warm for 4 hours, and obtain silicon-carbon powder after cooling;

[0048] The preparation method of the porous biomass carbon powder is as follows: 200g of hydrogen peroxide is dissolved in 2L of water, heated to 100°C, 100g of rice husk is added, and then 20mL of acetic acid is dripped into it and continued to heat at 100°C for 12h, and then washed with water and dried after cooling to obtain a biomass precursor; 100g of sodium hydroxide is mixed with 50g of biomass precursor and ground for 10h, transferred to an argon atmosphere and calcined at 700°C for 4h, and then washed with hydrochloric acid, washed with water, and dried to obtain a specific surface area of ​​2000cm 2 / g~2500cm 2 / g porous biochar powder;

[0049] S2, after mixing the silicon-carbon powder with the phenolic resin precursor solution, stirring and polymerizing at 80°C for 12 hours, collecting the precipitate, transferring it to a tubular furnace and calcining it at 700°C for 4 hours under argon conditions to obtain a biomass-based silicon-carbon negative electrode material;

[0050] The phenolic resin precursor solution is obtained by dissolving resorcinol and acetaldehyde in a mixed solvent at a molar ratio of 1:1, and the mixed solvent is composed of an aqueous solution of oxalic acid with a concentration of 2M and ethanol at a volume ratio of 1:2.

[0051] In the biomass-based silicon-carbon negative electrode material obtained above, the mass of silicon accounts for 53% of the total mass of the material.

[0052] The obtained biomass-based silicon-carbon negative electrode material and metal lithium were used to form a half-cell for electrochemical performance testing, with a test rate of 0.1C (first time) + 0.5C (cycle) and a charge and discharge voltage of 0.005-0.8V. The results showed that the discharge capacity of the negative electrode sheet can reach 1625.6mAh / g, with a first efficiency of 81.9%.

[0053] The obtained biomass-based silicon-carbon negative electrode material was evenly mixed with graphite in a mass ratio of 5:95 as a composite negative electrode material. NCM622 was used as the positive electrode, and the processes of slurry mixing, coating, rolling, slitting, die-cutting, lamination, welding of pole ears, top and side sealing, baking, and liquid injection were carried out to assemble 7Ah soft-pack batteries. After the batteries were divided into capacities, they were subjected to room temperature cycle tests at a current density of 1C / 1C. The initial efficiency of the battery cell was 84.9%. After 500 cycles of the full battery, the capacity retention rate was 92.1%.

[0054] Example 3

[0055] Preparation of biomass-based silicon-carbon anode materials:

[0056] S1. Place the porous biomass carbon powder in a rotary kiln, introduce argon gas for replacement for 1 hour, then heat to 500°C at a heating rate of 3°C / min, introduce tetrafluorosilane and keep warm for 3 hours, and obtain silicon-carbon powder after cooling;

[0057] The preparation method of the porous biomass carbon powder is as follows: 200g of sodium chlorate is dissolved in 3L of water, heated to 100°C, 200g of corn leaves are added, and then 30mL of acetic acid is dripped into it and continued to heat at 100°C for 12h, and then washed with water and dried after cooling to obtain a biomass precursor; 100g of potassium hydroxide is mixed with 100g of the biomass precursor and ground for 10h, transferred to an argon atmosphere and calcined at 800°C for 4h, and then washed with hydrochloric acid, washed with water, and dried to obtain a specific surface area of ​​1500cm 2 / g~1700cm 2 / g porous biochar powder;

[0058] S2, after mixing the silicon-carbon powder with the phenolic resin precursor solution, stirring and polymerizing at 60°C for 12 hours, collecting the precipitate, transferring it to a tubular furnace and calcining it at 800°C under argon conditions for 4 hours to obtain a biomass-based silicon-carbon negative electrode material;

[0059] The phenolic resin precursor solution is obtained by dissolving m-cresol and formaldehyde in a mixed solvent at a molar ratio of 1:2, and the mixed solvent is composed of a 2M phosphoric acid aqueous solution and ethanol at a volume ratio of 1:2.

[0060] In the biomass-based silicon-carbon negative electrode material obtained above, the mass of silicon accounts for 47% of the total mass of the material.

[0061] The obtained biomass-based silicon-carbon negative electrode material and metal lithium were used to form a half-cell for electrochemical performance testing, with a test rate of 0.1C (first time) + 0.5C (cycle) and a charge and discharge voltage of 0.005-0.8V. The results showed that the discharge capacity of the negative electrode sheet can reach 1613.9mAh / g, with a first efficiency of 80.2%.

[0062] The obtained biomass-based silicon-carbon negative electrode material was evenly mixed with graphite in a mass ratio of 5:95 as a composite negative electrode material. NCM622 was used as the positive electrode, and the processes of slurry mixing, coating, rolling, slitting, die cutting, lamination, electrode ear welding, top and side sealing, baking, and liquid injection were carried out to assemble a 7Ah soft-pack battery. After the battery was divided into capacities, a room temperature cycle test was carried out at a current density of 1C / 1C. The initial efficiency of the battery cell was 84.2%. After 500 cycles of the full battery, the capacity retention rate was 89.2%.

[0063] Comparative Example 1

[0064] Preparation of silicon-carbon negative electrode material:

[0065] S1. Commercially available porous carbon powder (specific surface area: 2053 cm 2 / g) was placed in a rotary furnace, argon was introduced for replacement for 1 hour, and then the temperature was increased to 550°C at a heating rate of 5°C / min, monosilane was introduced and kept warm for 4 hours, and silicon-carbon powder was obtained after cooling;

[0066] S2, after mixing the silicon-carbon powder with the phenolic resin precursor solution, stirring and polymerizing at 80°C for 12 hours, collecting the precipitate, transferring it to a tubular furnace and calcining it at 700°C for 4 hours under argon conditions to obtain a biomass-based silicon-carbon negative electrode material;

[0067] The phenolic resin precursor solution is obtained by dissolving resorcinol and acetaldehyde in a mixed solvent at a molar ratio of 1:1, and the mixed solvent is composed of an aqueous solution of oxalic acid with a concentration of 2M and ethanol at a volume ratio of 1:2.

[0068] The obtained silicon-carbon negative electrode material and metallic lithium were used to form a half-cell for electrochemical performance testing, with a test rate of 0.1C (first time) + 0.5C (cycle), and a charge and discharge voltage of 0.005-0.8V. The results show that the discharge specific capacity of the negative electrode plate can reach 1590.1mAh / g, and the first efficiency is 79.8%. It can be seen that compared with Example 2, Comparative Example 1 uses the porous biomass carbon prepared in Example 2 as a matrix and the silicon-carbon material obtained by silane deposition has a higher half-cell capacity and first efficiency. This is because the porous biomass carbon material obtained by the present invention has a narrow pore size range, which is more conducive to the deposition of silicon, so the amount of silicon deposition is large, and the nano-silicon is better combined with the carbon matrix, which is conducive to performance.

[0069] The obtained silicon-carbon negative electrode material and graphite are mixed evenly in a mass ratio of 5:95 as a composite negative electrode material, and NCM622 is used as the positive electrode. The 7Ah soft-pack battery is assembled by slurry mixing, coating, rolling, slitting, die cutting, lamination, welding pole ears, top side sealing, baking, and injection. After the capacity is divided, the normal temperature cycle test is carried out at a current density of 1C / 1C. The first efficiency of the battery cell is 83.1%, and the capacity retention rate is 86.5% after 500 cycles of the full battery. It can be seen that compared with Example 2, the silicon-carbon material obtained by silane deposition using the biomass carbon prepared in Example 2 as the matrix has a higher first efficiency of the battery cell and better full battery cycle performance. This is because the porous biomass carbon material obtained by the present invention has a more uniform pore distribution, so the nano-silicon of the silicon-carbon material obtained by the present invention is more evenly distributed in the carbon matrix, which is more conducive to alleviating volume expansion during the silicon lithium insertion process, so the cycle performance is better.

[0070] Comparative Example 2

[0071] Preparation of biomass-based silicon-carbon anode materials:

[0072] S1. Place the porous biomass carbon powder in a rotary kiln, introduce argon gas for replacement for 1 hour, then heat to 550°C at a heating rate of 5°C / min, introduce monosilane and keep warm for 4 hours, and obtain silicon-carbon material after cooling;

[0073] The porous biomass carbon powder was prepared by mixing 100 g of sodium hydroxide and 50 g of rice husk and grinding them for 10 h, transferring them to an argon atmosphere and calcining them at 700 °C for 4 h, then washing them with hydrochloric acid, washing them with water, and drying them to obtain a porous biomass carbon powder with a specific surface area of ​​1200 cm 2 / g~1500cm 2 / g porous biochar powder;

[0074] S2, after mixing the silicon-carbon material with the phenolic resin precursor solution, stirring and polymerizing at 80°C for 12 hours, collecting the precipitate, transferring it to a tubular furnace and calcining it at 700°C for 4 hours under argon conditions to obtain a biomass-based silicon-carbon negative electrode material;

[0075] The phenolic resin precursor solution is obtained by dissolving resorcinol and acetaldehyde in a mixed solvent at a molar ratio of 1:1, and the mixed solvent is composed of an aqueous solution of oxalic acid with a concentration of 2M and ethanol at a volume ratio of 1:2.

[0076] The obtained biomass-based silicon-carbon negative electrode material and metallic lithium were used to form a half-cell for electrochemical performance testing, with a test rate of 0.1C (first time) + 0.5C (cycle), and a charge and discharge voltage of 0.005-0.8V. The results show that the discharge specific capacity of the negative electrode plate can reach 1537.5mAh / g, and the first efficiency is 79.2%. It can be seen that compared with Example 2, Comparative Example 2 uses the porous biomass carbon prepared by selectively oxidizing and activating the biomass in Example 2 as a matrix and the silicon-carbon material obtained by silane deposition has a higher half-cell capacity and first efficiency. This is because the porous biomass carbon prepared by the selective oxidation and activation of the biomass in the present invention has a larger specific surface area and a narrower pore size range, which is more conducive to the performance.

[0077] The obtained biomass-based silicon-carbon negative electrode material and graphite are mixed evenly in a mass ratio of 5:95 as a composite negative electrode material, and NCM622 is used as the positive electrode. The 7Ah soft-pack battery is assembled by slurrying, coating, rolling, slitting, die-cutting, lamination, welding pole ears, top side sealing, baking, and injection. After the capacity is divided, the normal temperature cycle test is carried out at a current density of 1C / 1C. The first efficiency of the battery cell is 82.8%, and the capacity retention rate is 87.5% after 500 cycles of the full battery. It can be seen that compared with Example 2, the porous biomass carbon prepared by selective oxidation and activation treatment of biomass in Example 2 is used as the silicon-carbon material obtained by silane deposition. The first efficiency of the battery cell is higher, and the full battery cycle performance is better. This is because the porous biomass carbon material obtained by the present invention has a larger specific surface area and a more uniform pore distribution. Therefore, the nano-silicon of the silicon-carbon material obtained by the present invention is more evenly distributed in the carbon matrix, which is more conducive to alleviating volume expansion during the silicon lithium insertion process, so the cycle performance is better.

[0078] Comparative Example 3

[0079] Preparation of biomass-based silicon-carbon anode materials:

[0080] The porous biomass carbon powder was placed in a rotary kiln, argon was introduced for replacement for 1 hour, and then the temperature was raised to 550°C at a heating rate of 5°C / min, monosilane was introduced and kept warm for 4 hours, and the silicon-carbon negative electrode material was obtained after cooling;

[0081] The preparation method of the porous biomass carbon powder is as follows: 200g of hydrogen peroxide is dissolved in 2L of water, heated to 100°C, 100g of rice husk is added, and then 20mL of acetic acid is dripped into it and continued to heat at 100°C for 12h, and then washed with water and dried after cooling to obtain a biomass precursor; 100g of sodium hydroxide is mixed with 50g of biomass precursor and ground for 10h, transferred to an argon atmosphere and calcined at 700°C for 4h, and then washed with hydrochloric acid, washed with water, and dried to obtain a specific surface area of ​​2000cm 2 / g~2500cm 2 / g porous biomass carbon powder.

[0082] The obtained biomass-based silicon-carbon negative electrode material and metallic lithium were used to form a half-cell for electrochemical performance testing, with a test rate of 0.1C (first time) + 0.5C (cycle), and a charge and discharge voltage of 0.005-0.8V. The results showed that the discharge specific capacity of the negative electrode plate can reach 1613.5mAh / g, and the first efficiency is 77.6%. It can be seen that compared with Example 2, the half-cell capacity and first efficiency of the silicon-carbon material coated with phenolic resin carbon in Example 2 are higher in Comparative Example 3. This is because the use of phenolic resin carbon coating can modify the porous surface, reduce the occurrence of side reactions, and improve conductivity.

[0083] The obtained biomass-based silicon-carbon negative electrode material and graphite were mixed evenly in a mass ratio of 5:95 as a composite negative electrode material, and NCM622 was used as the positive electrode. The 7Ah soft-pack battery was assembled by slurry mixing, coating, rolling, slitting, die cutting, lamination, welding pole ears, top side sealing, baking, and injection. After the capacity was divided, the normal temperature cycle test was carried out at a current density of 1C / 1C. The first efficiency of the battery cell was 81.7%, and the capacity retention rate was 82.3% after 500 cycles of the full battery. It can be seen that compared with Example 2, the silicon-carbon material coated with phenolic resin carbon in Example 2 has a higher first efficiency of the battery cell and better full battery cycle performance. This is because the use of phenolic resin carbon coating can modify the porous surface, improve the conductivity, and protect the internal nanostructure and reduce contact with the electrolyte.

[0084] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a biomass-based silicon-carbon negative electrode material, characterized in that: The steps include: S1. Place the porous biomass carbon powder in a reaction furnace, introduce silicon source gas under an inert atmosphere, and calcine at a high temperature of 450° C. to 700° C. for 2 to 8 hours to obtain silicon carbon powder; The method for preparing the porous biomass carbon powder comprises: heating the biomass raw material in an oxidant solution under acidic conditions to obtain a biomass precursor; The biomass precursor is mixed with an activator and ball-milled, and then calcined at 700° C. to 900° C. for 1 to 8 hours under an inert atmosphere to obtain a product; S2, mixing the silicon-carbon powder and the phenolic resin precursor solution, heating and stirring to polymerize, and then separating the solid and the liquid, and sintering the obtained solid material at a high temperature of 600° C. to 800° C. for 4 to 6 hours under an inert atmosphere to obtain the obtained solid material.

2. The method for preparing the biomass-based silicon-carbon negative electrode material according to claim 1, characterized in that: In the method for preparing the porous biomass carbon powder, the mass ratio of the biomass raw material to the oxidant is 200-500:100-500; and the concentration of the oxidant solution is 10-200 g / L.

3. The biomass-based silicon-carbon negative electrode material and the preparation method thereof according to claim 1, characterized in that: In the method for preparing the porous biomass carbon powder, the temperature of the heating treatment under acidic conditions is 60 to 100° C. and the time is 8 to 12 hours.

4. The biomass-based silicon-carbon negative electrode material and the preparation method thereof according to claim 1, characterized in that: In the method for preparing the porous biomass carbon powder, the mass ratio of the biomass precursor to the activator is 1:1 to 1:

6.

5. The biomass-based silicon-carbon negative electrode material and the preparation method thereof according to claim 1, characterized in that: In S2, the conditions for the heating and stirring polymerization are: stirring polymerization at 60°C to 100°C for 8 to 12 hours.

6. The biomass-based silicon-carbon negative electrode material according to claim 1, characterized in that: The specific surface area of ​​the porous biomass carbon powder is 1000 cm 2 / g~3500cm 2 / g.

7. A biomass-based silicon-carbon negative electrode material, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 6.

8. The biomass-based silicon-carbon negative electrode material according to claim 7, characterized in that: In the biomass-based silicon-carbon negative electrode material, the mass of silicon accounts for 30% to 60% of the total mass of the material.

Citation Information

Patent Citations

  • China-hemp-based hierarchical pore carbon material as well as preparation method and application thereof

    CN111547723A

  • Silicon-carbon composite negative electrode material and preparation method and application thereof

    CN114068901A

  • Biomass-based porous carbon and preparation method thereof

    CN116924396A

  • Negative electrode material, preparation method thereof and battery

    CN117525353A