Preparation method and application of recyclable mineral-based carbon spheres based on agricultural wastes

By preparing reusable ore-based carbon balls based on magnesium-modified peanut shells based on agricultural waste, the problem of poor interception effect and high cost of water interception fillers on phosphorus is solved, and low-cost and efficient nitrogen and phosphorus adsorption and resource circulation are achieved. use.

CN118925671AActive Publication Date: 2024-11-12JIANGSU ACAD OF AGRI SCI +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411291161.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-12
Estimated Expiration
2044-09-14

AI Technical Summary

Technical Problem

The existing water intercepting filler has poor intercepting effect on phosphorus and is costly, and the processing problems after saturation affect resource recycling.

Method used

Reusable ore-based carbon balls are prepared using magnesium-modified peanut shells based on agricultural waste, and the peanut shells are modified by magnesium salt and KOH solution, and granulated and calcined in combination with starch, potassium bicarbonate, concave and convex rod soil and bauxite. , ore-based carbon balls with high specific surface area and strength are formed to adsorb nitrogen and phosphorus contaminants and return to aerobic compost after saturation.

Benefits of technology

It realizes low-cost and efficient intercepting of nitrogen and phosphorus pollutants, reduces the cost of filling production and treatment, and achieves safe reuse of resources through compost reuse.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925671A_ABST
    Figure CN118925671A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of adsorption materials, and relates to a preparation method and application of recyclable mineral-based carbon spheres based on agricultural waste, and the preparation method comprises the following steps: preparation of magnesium modified peanut shells: modifying and loading crushed peanut shells by using a magnesium salt solution, and then adding a KOH solution for treatment to obtain the magnesium modified peanut shells; the preparation method comprises the following steps: preparing recyclable mineral-based carbon spheres: mixing magnesium modified peanut shells, starch, potassium bicarbonate, attapulgite, bauxite and water, granulating and balling, and preheating at 150-200 DEG C for 1-2.5 hours after balling to form pores; and after preheating is completed, continuously calcining for 0.5-1.5 hours under the condition of 500-700 DEG C, and cooling to form the recyclable ore-based carbon spheres. The mineral-based carbon spheres are used for intercepting or adsorbing nitrogen and phosphorus in farmland recession in a fertilization period and / or a rainstorm period; and after completing saturated adsorption on nitrogen and phosphorus, the adsorbent can be reused for aerobic composting to increase soil fertility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of adsorption materials and relates to a preparation method of reusable mineral-based carbon balls based on agricultural waste and application thereof. Background Art

[0002] Nitrogen and phosphorus are the most important limiting factors for plant growth. Agricultural fertilization, industrial production, livestock and poultry breeding, and residents' lives produce a large amount of nitrogen and phosphorus-containing wastewater, some of which are directly or indirectly discharged into rivers, lakes, reservoirs, and seawater without treatment. They are important growth limiting factors for algae in rivers and lakes, and are also important inducements for eutrophication of water bodies, which can then cause ecological disasters such as algal blooms and blue algae outbreaks. A typical case is the Taihu blue algae incident in 2007. Therefore, my country's "Surface Water Environmental Quality Standards" set the water quality standards for ammonia nitrogen, total nitrogen, and total phosphorus as 2.0 mg / L, 2.0 mg / L, and 0.4 mg / L (Class V water) respectively, in order to control the input of nitrogen and phosphorus nutrients in surface water bodies into lakes and reservoirs. Therefore, controlling nitrogen and phosphorus in water bodies has important practical and strategic significance for controlling water environment improvement, water eutrophication control, and water ecosystem health.

[0003] At present, the interception fillers for pollutants in water bodies are mainly zeolite, aerated concrete, volcanic rock, etc. They mainly rely on their own rich pore structure and adsorption sites to achieve physical or chemical adsorption of nitrogen and phosphorus. However, the above interception fillers are generally not effective for phosphorus interception. The main reason is that phosphorus presents the same negative charge as the above fillers and has a small pore structure. Therefore, it is necessary to develop a new type of interception filler for nitrogen and phosphorus pollution. In the actual interception process, the cost of the filler is also an important factor. The expensive price is another important limiting factor that hinders the large-scale application of interception fillers. Therefore, the pursuit of a low-price strategy for interception fillers is of great significance for its mass production and promotion and application.

[0004] In addition, how to deal with saturated fillers is still a thorny issue. Simple stacking will occupy a large amount of land, and the threat of its leachate or degradation products to the soil cannot be ignored. Therefore, the development of recyclable fillers is of great significance for resource recycling. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing recyclable mineral-based carbon balls based on agricultural waste and its application.

[0006] The first aspect of the present invention provides a method for preparing recyclable mineral-based carbon balls based on agricultural waste, comprising the following steps:

[0007] Preparation of magnesium-modified peanut shells: using a magnesium salt solution to spray and modify the crushed peanut shells, and then spraying a KOH solution to modify the shells to obtain magnesium-modified peanut shells;

[0008] Preparation of recyclable mineral-based carbon spheres: magnesium-modified peanut shells, starch, potassium bicarbonate, attapulgite, bauxite, and water are mixed in proportion, granulated into spheres, and preheated at 150°C-200°C for 1h-2.5h (to form pores) after spheres are formed; after preheating, calcined at 500°C-700°C for 0.5h-1.5h, and cooled to form recyclable mineral-based carbon spheres;

[0009] The mass ratio of magnesium-modified peanut shell, starch, potassium bicarbonate, attapulgite, bauxite and water is 35:(1-3):(1-3):(35-45):(4-6):(15-25);

[0010] The total added molar ratio of magnesium ions in the magnesium salt solution and hydroxide ions in the KOH solution is: 1:(2.3-2.7).

[0011] In a preferred embodiment, during the preparation of magnesium-modified peanut shells, the crushed peanut shells are sieved, and the peanut shells are sprayed with a 0.2-1.5 mol / L magnesium salt solution so that the surface of the peanut shells is evenly moistened with the magnesium salt solution. After standing for 18-28 h (preferably 24 h), the peanut shells are evenly sprayed with a 1-2 mol / L KOH solution, and then stirred to mix.

[0012] Furthermore, the total molar ratio of magnesium ions in the magnesium salt solution and hydroxide ions in the KOH solution is 1:2.5; and the magnesium salt is MgCl2.

[0013] In a preferred embodiment, magnesium modification and pyrolysis are performed to cause the pores of peanut shells to swell and form nano-sized magnesium oxide MgO.

[0014] Preferably, after pelletizing, the pellets are preheated using the recovered heat from carbonization.

[0015] In a preferred embodiment, the recyclable mineral-based carbon sphere has a specific surface area of ​​>150 m 2 / g, fixed carbon>30%, iodine value>600mg / g, compressive strength of 5-10MPa, methylene blue value>100mg / g; the particle size of mineral-based carbon balls is 2-10mm.

[0016] More specific preparation steps are:

[0017] Preparation of Mg-modified peanut shells: The crushed peanut shells are sieved through a 60-mesh sieve, and the peanut shells are sprayed with a 0.5 mol / L MgCl2 solution. While spraying, a stirring device is used to mix and stir until the surface of the peanut shells is evenly wetted. Generally speaking, 100 kg of peanut shells can be spread out, and the spraying speed is 10 L / h, and the spraying time is about 10 minutes. After standing for a long time (preferably overnight), a 1.25 mol / L KOH solution (the concentrations of MgCl2 and KOH can be adjusted within a certain range, but the molar ratio of 1:2.5 must be maintained) is used to spray evenly according to the steps of spraying MgCl2. The spraying speed and spraying time are consistent with those of spraying MgCl2. The two reagents are sprayed alternately twice. After the spraying is completed, a stirrer is used to slowly stir and mix for 1-2 hours.

[0018] Preparation of recyclable mineral-based carbon balls: The raw materials include magnesium-modified peanut shells, starch, potassium bicarbonate, attapulgite, and bauxite. When preparing mineral-based carbon balls, the raw material ratio (weight parts) is 35 parts of magnesium-modified peanut shells, 2 parts of starch, 2 parts of potassium bicarbonate, 40 parts of attapulgite (as a binder) + 5 parts of bauxite (as a filler skeleton). After all the raw materials are fully stirred, 20 parts of water are added to perform disc granulation into balls (ball diameter 0.2-1cm, ball forming time is about 30min). After balling, the recovered heat of carbonization is used for preheating (to achieve pre-reaction between raw materials), the temperature is 150℃-200℃, and it lasts for 2h, and then it is fired in a carbonization kiln, the temperature is 500℃-700℃, and it lasts for 1h. After natural cooling, the required mineral-based carbon balls are formed, and its related parameters (such as elemental composition, porosity, strength) are as follows: specific surface area>150m 2 / g, fixed carbon>30%, iodine value>600mg / g, compressive strength 5-10MPa, methylene blue value>100mg / g.

[0019] Furthermore, the starch absorbs water and expands the original pore structure of the peanut shell. During preheating, potassium bicarbonate decomposes and dehydrates to form a pore structure. During calcination, starch pyrolyzes to form a pore structure, and bauxite decomposes, dehydrates and recrystallizes to form a hardened skeleton. When the peanut shell biochar completes the pyrolysis process, the MgO structure formed by the pyrolysis of Mg(OH)2 is loaded in the porous structure of the biochar.

[0020] The second aspect of the present invention discloses recyclable mineral-based carbon spheres obtained by the aforementioned preparation method.

[0021] The third aspect of the present invention provides an interception dam filled with the aforementioned recyclable mineral-based carbon balls.

[0022] Preferably, the interception dam is used to intercept or adsorb nitrogen and phosphorus in farmland runoff during fertilization and / or rainstorm periods; when the reusable mineral-based carbon balls have completed saturated adsorption of nitrogen and phosphorus, they can be reused for aerobic composting to increase soil fertility.

[0023] The fourth aspect of the present invention discloses the use of the aforementioned preparation method or the aforementioned recyclable mineral-based carbon balls in intercepting or adsorbing nitrogen and phosphorus in farmland runoff water.

[0024] The fifth aspect of the present invention discloses a method for treating mineral-based carbon balls after adsorption saturation for aerobic composting and reuse, adding 5-10% by mass of carbon ball powder (referring to the mass ratio of the mineral-based carbon ball powder after adsorption saturation to the mass ratio of the initial compost material composed of wheat straw and chicken manure), the wet weight of the initial compost material is 8.0 kg, and the ratio (mass ratio) of wheat straw: chicken manure = 1:1.5 is uniformly mixed. The water content is adjusted to about 60.0%. The composting process starts with the mixing of raw materials, and the compost is turned 4 times during the entire composting process. The compost is turned on the 11th, 16th, 24th, and 33rd days, and the composting is completed on the 36th day. When turning the compost, pour out the compost in the incubator and stir it evenly in a mixer. When stirring, add an appropriate amount of water to keep the water content of the compost at 55.0%-60.0%. Finally, the finished compost is obtained.

[0025] Compared with the prior art, the present invention has the following significant advantages:

[0026] The production process of the mineral-based carbon balls of the present invention is simple and convenient, and the required reagents such as MgCl2 and KOH are inexpensive. KOH and MgCl2 are preferably used as spraying reagents. Compared with alkaline reagents such as NaOH, the purpose of selecting KOH is mainly because K, as the main essential element for crops, can promote the growth of crops; compared with MgNO3, the main reason for selecting MgCl2 is that it has a significant price advantage. On the other hand, the residual metal chloride is more easily decomposed than oxides and sulfides.

[0027] More importantly, the spray wetting process can effectively save chemical reagents, reduce the reagent waste caused by solution impregnation or solution co-precipitation, and reduce the environmental problems and preparation costs caused by reagent treatment.

[0028] According to the spraying ratio of 1:2.5, Mg 2+ Theoretically, the concentration ratio of the two reactions is 1:2. However, since the two are sprayed alternately (MgCl2 is sprayed first, and then KOH is sprayed, which is conducive to the formation of MgO) to achieve surface co-precipitation reaction, there is Mg 2+In the case of incomplete reaction, therefore, sufficient OH- is provided to enable the above coprecipitation reaction to proceed completely. Through optimal experiments, the applicant of the present invention found that a ratio of 1:2.5 (molar ratio) (i.e., sufficient KOH) can promote the complete reaction, thereby promoting the formation of Mg(OH)2 products cross-linked inside the peanut shell. The modification process of MgCl2 and KOH can increase the number of surface adsorption sites of carbon spheres and improve the retention capacity for pollutants.

[0029] The metal loading, agricultural waste raw materials and their addition amount of this product are determined through a large number of experiments. After analyzing different metal loadings (Mg, Fe, Ca, La), as well as agricultural waste such as wheat straw, rice straw, peanut shells, corn cobs, yellow calamus, poplar sawdust and coffee grounds, through cross-validation analysis, it was concluded that peanut shell loading Mg can achieve the maximum nitrogen and phosphorus adsorption. The peanut shell material buried underground is loose and breathable, with rich pores, and has an interconnected pore structure that other biological wastes do not have. Through Mg modification, widely distributed Mg oxide components can be formed in its pores during the pyrolysis process. These Mg oxide components formed in the pores have also been shown to form nano-scale MgO structures through swelling, thereby expanding the original pores of the peanut shell (that is, MgO and water vapor formed by pyrolysis of Mg(OH)2 can expand the channels of biochar and promote the cross-linking structure of the pores). The formed MgO can provide a large number of adsorption sites for phosphate and nitric nitrogen; after preheating and high-temperature pyrolysis, the network structure formed by the water absorption and expansion process of peanut shell biochar and MgO and the added starch and the pyrolysis and foaming process of potassium bicarbonate has a higher nitrogen and phosphorus binding capacity than traditional fillers such as carbon balls and zeolites.

[0030] my country is rich in bauxite resources, which has an outstanding price advantage. In addition, Al2O3 in bauxite can form crystalline components under high temperature conditions, which can improve the compressive resistance and durability of the filler, provide basic rigidity characteristics, and prevent the filler from being washed away in the water. Preferably, the mass ratio of bauxite is about 5%, because too high a bauxite ratio will make the carbon ball difficult to crush when it is composted and reused, and the nitrogen and phosphorus nutrients it has trapped are difficult to release, while too low a bauxite ratio will result in poor rigidity of the carbon ball, which will be broken and cracked when used in a flowing water environment.

[0031] The present invention uses low-cost pore-forming agents starch and potassium bicarbonate, and the pore structure and gas generated by water absorption and pyrolysis can generate a large number of effective pore structures during the preheating process, thereby increasing the specific surface area of ​​the carbon sphere. The starch absorbs water and expands the original pore structure of the peanut shell. During preheating, potassium bicarbonate decomposes and dehydrates to form a pore structure; during calcination, starch pyrolyzes to form a pore structure.

[0032] Attapulgite is a natural clay mineral, and its main structure is a crystalline hydrated magnesium aluminum silicate mineral. Its micropores and pore structure have a large specific surface area and cation exchange capacity, and have considerable adsorption and interception capabilities for pollutants.

[0033] The preheating temperature is set at 150℃-200℃ for 2h, potassium bicarbonate decomposes and dehydrates, and promotes the formation of internal pore structure. The calcination temperature of mineral-based carbon balls is 500-700℃. Bauxite decomposes, dehydrates and recrystallizes at this temperature stage to form a hardened carbon ball skeleton. Biochar completes high pyrolysis, Mg(OH)2 pyrolyzes to form abundant MgO adsorption sites, and starch decomposes and carbonizes to form a pore structure. Higher temperatures may cause the cross-linked pore structure of biochar to begin to collapse, while lower pyrolysis temperatures make it difficult for bauxite to dehydrate and decompose, weakening its rigidity; or starch decomposition and carbonization are insufficient.

[0034] The mineral-based carbon balls of the present invention have better nitrogen and phosphorus interception effects than similar modified biochars, while the cost is only about 1 / 3-1 / 2 of that of similar modified biochars.

[0035] After the mineral-based carbon balls of the present invention are saturated with adsorption, they can be used for composting and reuse after safety assessment, thereby achieving safe reuse of nitrogen and phosphorus resources. The main components, MgO, attapulgite, biochar, bauxite, starch, potassium bicarbonate, etc., can be applied to the soil. They can provide the necessary nutrient supply for crops in combination with the fixed nitrogen and phosphorus pollutants, and can achieve a slow-release effect of nutrient release. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 The SEM images of the mineral-based carbon spheres of Example 1 and Example 2;

[0037] Figure 2 The pore volume and specific surface area of ​​the carbon spheres, wherein: a and b correspond to Example 1, c and d correspond to Example 4, e and f correspond to Example 7, and g and h correspond to Example 8;

[0038] Figure 3 Infrared spectra of different mineral-based carbon balls, a corresponds to Example 8, b corresponds to Example 4, c corresponds to Example 7, and d corresponds to Example 1;

[0039] Figure 4 Changes in N, P, K, and total nutrients in compost samples;

[0040] Figure 5 The contents of humus, fulvic acid, humic acid and changes in HA / FA in various treated organic fertilizers. DETAILED DESCRIPTION

[0041] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.

[0042] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, instruments, etc. used in the following examples are all commercially available unless otherwise specified.

[0043] Example 1

[0044] The crushed peanut shells were passed through a 60-mesh sieve, and the peanut shells were sprayed with a 0.5 mol / L MgCl2 solution at a spraying rate of 0.1 L / (h*kg) (i.e., 0.1 L MgCl2 solution was sprayed per kg of crushed peanut shells per hour), and the spraying time was 10 min. A stirring device was used for mixing and stirring (200 rpm) while spraying. After standing overnight, a 1.25 mol / L KOH solution was used for uniform spraying in the same steps as spraying MgCl2. The spraying speed and spraying time were consistent with the steps of spraying MgCl2. The two reagents were sprayed alternately for 2 times. After the spraying was completed, a stirrer was used to stir (200 rpm) and mix for 1 hour. The magnesium-modified peanut shells were taken out and dried for later use.

[0045] Preparation of recyclable mineral-based carbon spheres:

[0046] 35 parts of magnesium-modified peanut shells, 2 parts of starch, and 2 parts of potassium bicarbonate are mixed in advance, and then 40 parts of attapulgite and 5 parts of bauxite are added. After being fully stirred, 20 parts of water are added and disc granulation is performed to form balls (ball diameter 0.2-1cm, ball forming time 30min). After balling, the recovered heat of carbonization is used for preheating at 150°C for 2h; then a carbonization kiln is used for calcination at a calcination temperature of 600° for 1h, and then the ball is naturally cooled to form the required mineral-based carbon balls 1.

[0047] Embodiment 2:

[0048] The preparation method is similar to that of Example 1, the only difference being the surface modification process without metal MgCl2 and KOH, and the product is mineral-based carbon sphere 2.

[0049] Embodiment 3:

[0050] The preparation method is similar to that of Example 1, except that no attapulgite is added, and the product is mineral-based carbon balls 3.

[0051] Embodiment 4:

[0052] The preparation method is similar to that of Example 1, except that peanut shells are replaced with rice straw, and the product is mineral-based carbon spheres 4.

[0053] Embodiment 5:

[0054] The preparation method is similar to that of Example 1, except that the impregnation method is used to prepare the relevant modified Mg biochar, and the product is mineral-based carbon ball 5.

[0055] Embodiment 6:

[0056] The preparation method is similar to that of Example 1, except that the types of metals sprayed are Fe (ferric chloride solution) and La (lanthanum chloride), and the products are mineral-based carbon balls 6 and 7, respectively.

[0057] Embodiment 7:

[0058] The preparation method is similar to that of Example 1, except that no potassium bicarbonate is added, and the product is mineral-based carbon sphere 8.

[0059] Embodiment 8:

[0060] The preparation method is similar to that of Example 1, except that no starch is added, and the product is mineral-based carbon sphere 9.

[0061] Embodiment 9:

[0062] The preparation method is similar to that of Example 1, except that there is no preheating process, and the product is mineral-based carbon sphere 10.

[0063] For the modified biochars made from different biomass raw materials (only the biomass materials were modified, not made into carbon balls), the phosphate adsorption rate of biochars modified with different metals was determined experimentally, and the suitable raw materials and modified metal types were analyzed and screened. The results are shown in Table 1.

[0064] Table 1 Adsorption rate (%) of modified biochar powder (0.5 g) prepared from different raw materials for phosphate (1 L, 10 mg / L)

[0065]

[0066] The data in Table 1 show that the peanut shell raw material has a much higher adsorption effect on phosphate after being modified with Mg than other raw materials and modified metal types. Therefore, preferably, peanut shell and Mg modification are the preferred conditions of the present invention.

[0067] like Figure 1 As shown, A corresponds to mineral-based carbon ball 1, and B corresponds to mineral-based carbon ball 2. Figure 1 The results show that compared with mineral-based carbon balls that have not been loaded with MgCl2 and KOH, the surface loading process can effectively increase the uneven pore structure of the material surface, thereby improving the material's ability to absorb pollutants.

[0068] Figure 2The results show that the replacement of magnesium-modified peanut shells with magnesium-modified rice straw, without the addition of starch and potassium bicarbonate, all lead to a significant reduction in the specific surface area and pore volume of carbon balls. In Example 1, the combined use of magnesium-modified peanut shells, starch and potassium bicarbonate can greatly increase the pore structure and specific surface area of ​​carbon balls, thereby improving the ability of carbon balls to reduce pollutants. This is mainly due to the fact that starch and potassium bicarbonate enter the loose and porous structure of peanut shells, and starch absorbs a certain amount of water to absorb water and expand, and the volume can reach dozens to hundreds of times the original. In the preheating stage, potassium bicarbonate acts as a foaming agent, thereby producing a large amount of carbon dioxide gas, which promotes the generation of pores in carbon balls, and the generated pores are also conducive to the further pyrolysis and expansion of starch, which plays a complementary role in improving the pores of carbon balls. In the calcination stage, the starch and peanut shells that enter the pores of the peanut shells undergo differential carbonization due to the different difficulty of pyrolysis, which further improves the porosity of the carbon balls. Therefore, in the invention, in the porous structure of peanut shells, the expansion and carbonization of starch combined with the foaming agent function of potassium bicarbonate can effectively improve the pore structure of carbon balls and achieve a synergistic effect.

[0069] Figure 3 The results show that the surface functional groups of the mineral-based carbon spheres with a complete formula have a richer functional group structure than those of other embodiments, while the mineral-based carbon spheres without other components lack the functional groups corresponding to specific bands, such as 750cm -1 Carbonate, a functional group, can fix nitrogen and phosphorus pollutants in water through ion exchange. Therefore, the use of multiple formulations can increase the abundance of functional groups on the filler surface, thereby providing more adsorption sites during the pollutant reduction process.

[0070] Application Example 1 Laboratory interception and purification experiment

[0071] The experimental water was artificially cultivated simulated polluted water: COD 30mg / L, total nitrogen 15mg / L, ammonia nitrogen (NH4 + -N)5mg / L, total phosphorus 1mg / L.

[0072] An adsorption device was constructed in the laboratory for testing. 50 g of the above different test fillers were added to 50 L of simulated wastewater, and the pH was maintained at 7.5 ± 0.2 at room temperature. After stirring and adsorbing for 24 hours, the changes in the content of different pollutants in the supernatant before and after adsorption were detected, and the adsorption removal rate was calculated accordingly. The results in Table 2 show that the surface Mg loading, attapulgite addition, peanut shell matrix, modified metal MgO, a certain preheating process, especially the synergistic combination of starch, potassium bicarbonate and peanut shells, can increase the purification capacity of mineral-based carbon balls for nitrogen and phosphorus in water.

[0073] In Example 5, since the impregnation method requires the use of a large-volume container to immerse the raw materials, the amount of waste liquid generated by the biochar using the impregnation method is about dozens of times that of the spraying method, that is, the use of the spraying method can greatly reduce the production cost.

[0074] The addition of bauxite can increase the mechanical strength of mineral-based carbon balls, making them more resistant to impact in ditch water.

[0075] Table 2 Adsorption of TN, ammonia nitrogen and TP by different mineral-based carbon balls

[0076] Adsorption rate (%) TN Ammonia nitrogen TP Mineral-based carbon ball 1 69.5 64.5 63.5 Mineral-based carbon ball 2 62.1 52.2 52.1 Mineral-based carbon ball 3 70.5 42.1 56.8 Mineral-based carbon ball 4 62.3 56.9 54.0 Mineral-based carbon ball 6 63.1 50.6 53.2 Mineral-based carbon ball 7 56.5 55.5 53.1 Mineral-based carbon ball 8 49.1 49.0 57.8 Mineral-based carbon ball 9 51.7 49.7 62.4 Mineral-based carbon ball 10 39.4 47.1 49.5

[0077] Application Example 2: Ditch interception and purification experiment

[0078] An interception dam filled with mineral-based carbon balls was set up in the actual ditch, and its interception effect on nitrogen and phosphorus in the farmland runoff during the fertilization period and the rainstorm period was monitored and analyzed. The dam was set up according to the addition amount of 0.01 cubic meter of filler per mu of rice field. The specific location is located in the farmland interception ditch in Zhaojiatang area, Xinkang Village, Wujin District, Changzhou, my country. The results are shown in Table 3.

[0079] Table 3 The interception effect of mineral-based carbon balls on nitrogen and phosphorus in farmland runoff during fertilization and rainstorm periods

[0080]

[0081]

[0082] Application Example 3 Adsorption Saturated Carbon Ball Composting Recycling Experiment

[0083] Four treatments were designed in this study: CK0 (control without addition), T1, T2 and T3. T1 is to add 10% adsorption saturated Mg modified peanut shell biochar powder; T2 is to add 10% adsorption saturated mineral-based carbon ball 1 powder obtained by crushing. In T3, the modified biochar ball, that is, the mineral-based carbon ball 1 prepared in Example 1, is reused after adsorption saturation (addition amount 10%). The mass fraction of 10% is the mass ratio of biochar powder or carbon ball to the mass ratio of the initial compost material.

[0084] Chicken manure is processed, crushed and passed through a 5mm sieve; wheat straw is processed and crushed to 1-2cm.

[0085] The composting reactor is a PP material insulation box with an inner diameter of 52.5×40×29 (cm) and an outer diameter of 64×48×36 (cm). The composting process lasts for 36 days. The initial wet weight of the composting material is 8.0 kg, and it is evenly mixed in a ratio of wheat straw: chicken manure = 1:1.5. The moisture content of wheat straw and chicken manure is 10.9% and 12.6%, respectively. The conditioner is mixed evenly with the compost, and the moisture content of each treatment is adjusted to about 60.0%. The composting process starts with the mixing of raw materials, and the compost is turned 4 times during the entire composting process. The compost is turned on the 11th, 16th, 24th, and 33rd days, and the composting is completed on the 36th day. When turning the compost, pour out the compost in the incubator and stir it evenly in a mixer. When stirring, add an appropriate amount of water to keep the moisture content of the compost at 55.0%-60.0%. After turning the compost, pour out the fertilizer in the mixer and put it into the original insulation box to continue composting. The agitator was cleaned three times with water, and then the next compost treatment was turned until all the treated composts were turned. Samples were collected after each turning. During the thermophilic phase and cooling phase of the compost, the moisture content of the compost was adjusted to 55.0-60.0% after each sampling. During the maturing period of the compost, no water was added during turning.

[0086] like Figure 4 As shown, the variation patterns of total nitrogen among the treatments were similar, with the highest content in the high temperature period (average value was 2.50%), gradually decreasing in the cooling period (average value was 2.00%), and slightly increasing in the maturity period (average value was 2.25%).

[0087] At the end of the maturity period, compared with the control group, the TK content in the T2 treatment increased by nearly 25% ( Figure 4 c), 50%-75% more than the high temperature heating period of CK0 treatment, but the TK content of T3 treatment did not change much (increased by about 1.2%); at the end of composting, the total nutrient content of the control group increased by 35.3%, the total nutrient content of T1 treatment increased by 35.7%, the total nutrient content of T2 treatment increased by 25%, and the total nutrient content of T3 treatment increased by 28.6%. The experimental results show that the total nutrients of the composting treatments with modified biochar powder (T2 treatment) and modified biochar balls (T3 treatment) are close to the total nutrients of T1.

[0088] The degree of humification can reflect the degree of biodegradation and the stability of compost products. Figure 5As shown in a, compared with the control group, the HA content of the T2 treatment (addition of Mg-modified biochar powder) increased (increased by 1.01%), and the HA content of the T1 and T3 treatments decreased slightly (decreased by 1.0%). Compared with the control, the humic acid / fulvic acid (HA / FA) ​​ratio of the T2 composting treatment was significantly higher, increasing by 2.2%, and there was no significant difference in the other composting treatments (p<0.05).

[0089] In summary, the addition of 10% adsorption saturated mineral-based carbon balls does not weaken the nitrogen and phosphorus nutrients in the compost, and helps to increase the degree of humification (HA / FA ratio). In particular, the use of modified saturated biochar crushed into powder in composting can maintain and improve the fertilizer efficiency of compost in the presence of exogenous material input, which is conducive to the recycling of adsorption saturated mineral-based carbon balls.

[0090] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the above embodiments do not limit the present invention in any form, and any technical solution obtained by equivalent replacement or equivalent transformation falls within the protection scope of the present invention.

Claims

1. A method for preparing recyclable mineral-based carbon balls based on agricultural waste, characterized in that: The steps include: Preparation of magnesium-modified peanut shells: using a magnesium salt solution to spray and modify the crushed peanut shells, and then adding a KOH solution to treat, to obtain magnesium-modified peanut shells; Preparation of recyclable mineral-based carbon spheres: Mix magnesium-modified peanut shells, starch, and potassium bicarbonate, then add attapulgite, bauxite, and water to mix, granulate into spheres, preheat at 150°C-200°C for 1h-2.5h after spheres are formed; after preheating, continue calcining at 500°C-700°C for 0.5h-1.5h, and cool to form recyclable mineral-based carbon spheres; The mass ratio of magnesium-modified peanut shell, starch, potassium bicarbonate, attapulgite, bauxite and water is 35:(1-3):(1-3):(35-45):(4-6):(15-25); The total added molar ratio of magnesium ions in the magnesium salt solution and hydroxide ions in the KOH solution is: 1:(2.3-2.7).

2. The method for preparing recyclable mineral-based carbon balls based on agricultural waste according to claim 1, characterized in that: In the preparation process of magnesium-modified peanut shells, the crushed peanut shells are sieved, and the peanut shells are sprayed with a 0.2-1.5 mol / L magnesium salt solution so that the surface of the peanut shells is evenly wetted by the magnesium salt solution. After standing for 18-28 hours, the peanut shells are evenly sprayed with a 1-2 mol / L KOH solution and then stirred to mix.

3. The method for preparing recyclable mineral-based carbon balls based on agricultural waste according to claim 1, characterized in that: The total molar ratio of magnesium ions in the magnesium salt solution and hydroxide ions in the KOH solution is 1:2.5; the magnesium salt is MgCl2.

4. The method for preparing recyclable mineral-based carbon balls based on agricultural waste according to claim 1, characterized in that: Through magnesium modification and pyrolysis, the pores of peanut shells swell to form nano-scale magnesium oxide MgO.

5. The method for preparing recyclable mineral-based carbon balls based on agricultural waste according to claim 1, characterized in that: The recyclable mineral-based carbon spheres have a specific surface area of ​​>150m 2 / g, fixed carbon>30%, iodine value>600mg / g, compressive strength of 5-10MPa, methylene blue value>100mg / g; the particle size of mineral-based carbon balls is 2-10mm.

6. The method for preparing recyclable mineral-based carbon balls based on agricultural waste according to claim 1, characterized in that: Starch absorbs water and expands to form a porous structure. During preheating, potassium bicarbonate decomposes and dehydrates to form a foaming structure. During calcination, magnesium-modified peanut shells are pyrolyzed to form biochar, starch decomposes and carbonizes to form a porous structure, and bauxite decomposes, dehydrates and recrystallizes to form a hardened skeleton. At the same time, during the pyrolysis of biochar, the sprayed Mg(OH)2 forms a rich MgO structure that is loaded in the porous structure of the biochar.

7. Recyclable mineral-based carbon spheres obtained by the preparation method according to any one of claims 1 to 6.

8. An interception dam, characterized in that: The interception dam is filled with the recyclable mineral-based carbon balls described in claim 7.

9. The interception dam according to claim 8, characterized in that: The interception dam is used to intercept or adsorb nitrogen and phosphorus in farmland runoff during fertilization and / or rainstorm periods; when the reusable mineral-based carbon balls have completed saturated adsorption of nitrogen and phosphorus, they can be crushed and reused in compost to increase soil fertility. The amount of mineral-based carbon balls added is 5-10% by mass.

10. Use of the preparation method according to any one of claims 1 to 6 or the recyclable mineral-based carbon balls according to claim 7 in intercepting or adsorbing nitrogen and phosphorus in farmland runoff.

Citation Information

Patent Citations

  • Preparation method of modified charcoal-based adsorbent for removing hydrogen sulfide

    CN105056882A

  • Construction method for multi-stage efficient interception and recycling of nitrogen and phosphorus pollution in farmland recession

    CN111533364A

  • High-starch-content bio-based porous activated carbon and preparation method thereof

    CN114735699A

  • Preparation process of agricultural and forestry waste-based biochar composite filter material

    CN116688647A

  • Multi-stage recycling method of magnesium modified carbon-based phosphorus adsorbent waste

    CN117720369A