Carbonate hydrogenation reduction zero-carbon decomposition method and system based on hydrogen combustion self-heating
Through the combination of hydrogen combustion self-heating and iron-containing catalyst, the problems of hydrogen supply molecules dilution and carbon emissions in the traditional carbonate calcination process are solved, and zero carbon emissions for carbonate decomposition and efficient utilization of iron-containing solid waste are achieved. , improves conversion efficiency and reaction rate, and has important industrial application prospects.
Patent Information
- Application Number
- CN202410986102.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-08
AI Technical Summary
In the traditional carbonate high-temperature calcination process, hydrogen supply molecules are diluted by nitrogen, with low conversion efficiency, large carbon emissions, and low utilization efficiency of iron-containing solid waste, making it difficult to achieve effective heating and zero carbon emissions for carbonate hydrolysis. .
Using the method of self-heating of hydrogen combustion, the mixture of hydrogen, oxygen and carbon dioxide is used to replace traditional air, and the iron-containing catalyst is used to promote the pyrolysis of carbonate and the in-situ conversion of CO2, and green hydrogen is prepared in combination with renewable energy to reduce carbon emissions. , and use iron-containing solid waste as a catalyst to increase the reaction rate and conversion rate.
It has achieved zero carbon emissions in the carbonate decomposition process, improved conversion efficiency and kinetic reaction rate, reduced energy consumption and carbon emissions, and has significant energy saving and emission reduction benefits and industrial application value.
Smart Images

Figure CN118908260A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field related to carbon reduction and efficiency improvement in carbonate calcination and decomposition processes in industries such as cement, steel, and refractory materials, as well as the technical field related to large-scale application of new energy green hydrogen and efficient comprehensive utilization of iron-containing solid waste. Specifically, it relates to a method and system for achieving zero-carbon decomposition of carbonates by self-heating through hydrogen combustion and catalytic hydrogenation of iron-containing solid waste. Background Art
[0002] High-temperature thermal decomposition of carbonates is a core process in cement, steel, refractory and other industries. In this process, carbonate decomposition produces CO 2 And fossil fuel combustion for heating emissions of CO 2 These two major sources of carbon emissions, therefore, need to develop targeted and effective carbon reduction and efficiency improvement solutions. 2 , CH 4 As hydrogen donor molecules (reducing agents), the CO2 reduction can be achieved by coupling the co-thermal decomposition of carbonates with the catalytic reduction of hydrogen donor molecules. 2 The in-situ hydrogenation conversion of 20% to 20% has a good industrial application prospect and extremely high ecological and economic value. Regarding this coupling process, relevant studies at home and abroad have verified the role of the introduction of hydrogen donor molecules in reducing the carbonate decomposition temperature and synergizing CO 2 The feasibility of conversion.
[0003] However, under the process conditions of traditional high-temperature carbonate calcination relying on coal-fired heating, if hydrogen molecules are directly introduced into the decomposition furnace, CO 2 and the hydrogen donor molecule will be N 2 (from the combustion air) is greatly diluted, which not only affects CO 2 The conversion efficiency of the hydrogen-donating molecules will also bring the burden of downstream product separation. Therefore, how to achieve effective heat supply in the carbonate hydrogenation decomposition reaction process under actual industrial production conditions is a difficulty faced by this process.
[0004] Hydrogen energy, as a green energy with high calorific value and multiple sources, is an important energy carrier in the future. Green hydrogen, as a green secondary energy, can be used as a fuel for high-temperature decomposition of carbonates to achieve zero carbon emissions in the heat supply link.
[0005] Bulk solid waste (hereinafter referred to as "solid waste") is a core area of comprehensive resource utilization, with large volume and wide coverage, prominent environmental impact and broad prospects for utilization. Promoting the comprehensive utilization of bulk solid waste is of great significance to improving resource utilization efficiency, improving environmental quality and promoting the comprehensive green transformation of economic and social development. The comprehensive utilization of bulk iron-containing solid wastes such as steel slag, fly ash, tailings, and smelting slag is still an industrial problem. Billions of tons of solid waste accumulation urgently need to find a way to make reasonable use of them. By adding iron-containing solid waste during the carbonate calcination and decomposition stage, CO of active iron species can be used. 2The hydrogenation catalytic activity promotes the reaction between hydrogen-donating molecules and carbonates. At the same time, the active free calcium oxide in the solid waste can be calcined at high temperature, which can solve the problem of poor mechanical properties of traditional steel slag cement.
[0006] In summary, a system and method is provided for calcining carbonates using excess green hydrogen as fuel gas and in-situ catalytic hydrogenation decomposition under the action of iron-containing solid waste to achieve zero-carbon decomposition in the carbonate refining process. This is not only of great significance for carbon reduction and efficiency improvement and resource utilization of bulk solid waste, but also has strong industrial application value. Summary of the invention
[0007] One of the purposes of the present invention is to provide a method for zero-carbon decomposition of carbonate by hydrogenation reduction based on self-heating of hydrogen combustion.
[0008] The second object of the present invention is to provide a system for carbonate hydrogenation reduction and zero-carbon decomposition based on hydrogen combustion self-heating.
[0009] The technical solution adopted by the present invention to achieve one of the purposes is to provide a method for zero-carbon decomposition of carbonate by hydrogenation reduction based on self-heating of hydrogen combustion, comprising the following steps: A mixed gas is formed by mixing hydrogen, oxygen and carbon dioxide in a volume ratio of (6-8): (1-1.5): (0.5-3); the mixed gas is introduced into a mixed system of a carbonate raw material and an iron-containing catalyst; under the catalytic action of the iron-containing catalyst, the carbonate is pyrolyzed by self-heating by combustion of part of the hydrogen, and the carbon dioxide generated by the pyrolysis of the carbonate is converted in situ by using the unburned hydrogen.
[0010] The general idea of the present invention is as follows: The present invention aims to solve the problems of traditional high-temperature calcination of carbonates that rely on coal-fired heating, such as the significant dilution of hydrogen molecules by nitrogen, low conversion efficiency, and high carbon emissions. The present invention provides a method for zero-carbon decomposition of carbonates by hydrogenation reduction based on self-heating of hydrogen combustion. The method uses hydrogen as an energy raw material for carbonate pyrolysis, and uses a mixture of hydrogen, oxygen, and carbon dioxide to replace the air atmosphere of the traditional carbonate calcination process. On the one hand, the self-heating of the combustion of part of the hydrogen is used to achieve the pyrolysis of carbonates, replacing the use of heat sources such as coal; on the other hand, excess unburned hydrogen is also used to convert carbon dioxide generated by carbonate pyrolysis in situ. In addition, the present invention incorporates a certain proportion of iron-containing catalyst into the carbonate raw material, which can utilize the potential CO 2 Hydrogenation catalytic activity to increase the kinetic reaction rate of carbonate decomposition and CO 2 The in-situ conversion rate also helps to achieve high-value utilization of iron-containing solid waste.
[0011] In the above method, the composition of the mixed gas is a key factor to ensure the safe and smooth progress of the pyrolysis of carbonates and the in-situ conversion of carbon dioxide. Since hydrogen combustion is a violent chain reaction, there are safety risks. If the gas ratio is improper, it will lead to serious consequences of explosion. After a lot of research and experiments, the present invention has determined that in the mixed gas, the volume ratio of hydrogen, oxygen and carbon dioxide is controlled to be in the range of (6-8): (1-1.5): (0.5-3). Among them, carbon dioxide gas, as a hydrogenation reaction gas, can absorb reaction heat, control the intensity of the combustion reaction, and avoid the combustion reaction from developing upstream of the intake pipe against the gas flow; adopting a hydrogen-oxygen ratio with excess hydrogen and controlling the proportion of oxygen in the mixed gas system to 10%-15% can reduce the risk of hydrogen deflagration. Under the above-mentioned ratio conditions, it can not only ensure the safe combustion and heat supply of hydrogen, but also achieve the purpose of further converting the unreacted carbon dioxide in the tail gas as a combustion control gas.
[0012] Furthermore, the hydrogen is prepared by renewable energy. Preferably, the hydrogen used in the present invention is green hydrogen prepared by renewable energy such as wind and light, which can reduce carbon emissions from the hydrogen supply source, thereby enhancing the overall carbon reduction efficiency of the carbonate hydrogenation process route. At the same time, the oxygen produced by the green hydrogen preparation process can also be used as an oxidant in the carbonate hydrogenation pyrolysis process.
[0013] Preferably, in the mixed gas, the volume ratio of hydrogen, oxygen and carbon dioxide is 7:(1-1.2):2.
[0014] Furthermore, the carbonate raw material includes one or more combinations of calcium carbonate, magnesium carbonate, ferrous carbonate, limestone, dolomite, marble, calcite, magnesite, and siderite.
[0015] Furthermore, the iron-containing catalyst comprises one or more combinations of iron-containing solid waste, active iron species extracted from iron-containing solid waste, or catalysts modified with iron-containing solid waste as a matrix.
[0016] Furthermore, the iron-containing solid waste includes a combination of one or more of red mud, steel slag, fly ash, coal gangue, and iron ore powder. In the present invention, adding cheap iron-containing solid waste as a catalyst to the carbonate raw material can achieve carbonate hydrogenation catalytic decomposition and CO at a lower temperature. 2 In-situ conversion has significant benefits in energy saving and emission reduction.
[0017] Preferably, the catalyst modified with iron-containing solid waste as the matrix comprises: a Fe-Al bimetallic catalyst prepared by a sol-gel method, wherein the molar fraction of the iron element in the catalyst is (40%-80%). 2 -CO 2Active iron species were precipitated by in-situ reduction in the atmosphere, showing excellent reverse water-gas shift (RWGS) reaction activity and promoting carbonate pyrolysis.
[0018] Furthermore, the mass ratio of the iron-containing catalyst to the carbonate raw material is 1: (5-20). Preferably, the mass ratio of the iron-containing catalyst to the carbonate raw material is 1: (8-12), which controls the iron content at a low level while satisfying good catalytic performance.
[0019] Furthermore, the carbon dioxide in the mixed gas includes unreacted carbon dioxide in the in-situ conversion.
[0020] Furthermore, the study found that the flow rate of the mixed gas and the feeding rate of the mixed system in the reactor will jointly affect the suspension state and residence time of the solid raw material in the reactor. When the volume mass ratio of the mixed gas to the mixed system (carbonate raw material and iron-containing catalyst) per unit time is controlled to be 1: (5-7) L / g, the residence time of the solid raw material in the reactor zone can be controlled to be 10-20s, so that the powder raw material particles can be decomposed in a suspended state in the reactor.
[0021] Preferably, the flow rate of the mixed gas is 1-5 L / min, and the feed rate of the mixed system is 0.1-0.5 g / s. By optimizing the flow rate of the mixed gas, higher hydrogen utilization and carbon dioxide conversion can be achieved, while maintaining the optimal flame temperature in terms of combustion and not easily causing flashback danger due to fluctuations in gas composition.
[0022] More preferably, the flow rate of the mixed gas is 2-3 L / min, and the feeding rate of the mixing system is 0.2-0.3 g / s, so that the powder raw material particles can obtain a more complete decomposition effect in the reactor.
[0023] Furthermore, the pyrolysis temperature of the carbonate is 600-1260°C.
[0024] In the present invention, hydrogen combustion self-heating is used to provide energy for the decomposition of carbonate. Since hydrogen combustion itself has a temperature field distribution of the flame, on the one hand, carbonate can be decomposed in a lower temperature zone, saving hydrogen fuel; on the other hand, there is a local high temperature zone (hydrogen flame) during the pyrolysis process, which is conducive to the endothermic reaction of carbon dioxide hydrogenation conversion, thereby improving the export conversion rate of carbon dioxide.
[0025] The technical solution adopted by the present invention to achieve the second purpose is to provide a system for carbonate hydrogenation reduction zero-carbon decomposition based on hydrogen combustion self-heating, and the method described in one of the purposes of the present invention. The system includes: a reactor body, a feed inlet, a discharge port, a mixed gas inlet, a calcined gas product outlet, and a CO 2 Circulation pipe.
[0026] Among them, CO 2 The setting of the circulation pipeline can use the unreacted carbon dioxide in a single pass as a circulating gas and apply it to the mixed intake air, achieving the dual purpose and effect of controlling combustion to improve system safety and fully converting carbon dioxide to reduce carbon emissions.
[0027] Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention provides a method and system for zero-carbon decomposition of carbonate hydrogenation reduction based on self-heating by hydrogen combustion. On the one hand, hydrogen is used as the fuel gas of the carbonate decomposition furnace to replace the traditional coal combustion energy supply mode, which can eliminate the carbon emissions generated by the high-temperature heating part; on the other hand, excess hydrogen is used as a hydrogen supply molecule for the carbonate hydrogenation decomposition reaction, which can realize the CO generated by carbonate decomposition. 2 In-situ conversion can theoretically achieve the goal of zero carbon emissions.
[0028] (2) The present invention provides a method and system for zero-carbon decomposition of carbonate by hydrogenation reduction based on self-heating of hydrogen combustion, in which iron-containing solid waste is added as a catalyst into carbonate raw materials, and the potential CO 2 Hydrogenation catalytic activity to increase the kinetic rate of carbonate decomposition and CO 2 In-situ conversion rate, at the same time, the added solid waste can partially replace the limestone raw materials, thereby realizing the high-value utilization of solid waste.
[0029] (3) The method and system provided by the present invention coordinate the process requirements of green hydrogen production from renewable energy, carbonate reduction decomposition, and comprehensive utilization of solid waste, and can ultimately achieve zero-carbon decomposition of carbonate hydrogenation reduction based on self-heating of hydrogen combustion, which has important practical significance and broad industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 A schematic diagram of the structure of a system for carbonate hydrogenation reduction and zero-carbon decomposition based on hydrogen combustion self-heating provided by the present invention; Among them, 1-reactor body; 2-feed port; 3-discharge port; 4-mixed gas inlet; 5-calcined gas product outlet; 6-CO 2 Circulation pipes; F1-carbonate raw material; F2-iron-containing solid waste; F3-metal oxide product; F4-mixed gas; F5-reaction gas product; F6-hydrogen; F7-oxygen; F8-gas product separation CO 2 . DETAILED DESCRIPTION
[0031] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0032] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0033] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited thereto.
[0034] Example 1 1 g of calcium carbonate powder was mixed with 100 mg of an iron-containing catalyst (Fe-Al bimetallic catalyst with a molar fraction of iron of 50%) and added to a glass tube reactor. H was introduced from the bottom. 2 :O 2 :CO 2 =700:100:200 ml / min of hydrogen-rich mixed gas was ignited at the gas inlet, and the carbonate reaction temperature was controlled at 700 by adjusting the gas flow rate and the height of the solid reactant raw material bed from the flame. o C. After running for 6 minutes, the solids were collected for thermogravimetric analysis of carbonate content, and the gas products entered the mass spectrometer for gas composition and concentration analysis. The results showed that the decomposition rate of calcium carbonate within 6 minutes was 72.1%, and CO 2 The in-situ conversion rate was 78.3%.
[0035] Example 2 1 g of calcium carbonate powder was mixed with 100 mg of steel slag powder and added to a glass tube reactor. H 2 :O 2 :CO 2 =700:110:200 ml / min of hydrogen-rich mixed gas was ignited at the gas inlet, and the carbonate reaction temperature was controlled at 700 by adjusting the gas flow rate and the height of the solid reactant raw material bed from the flame. o After running for 6 minutes, the solids were collected for thermogravimetric analysis of carbonate content, and the gas products entered the mass spectrometer for gas composition and concentration analysis. The results showed that the decomposition rate of calcium carbonate within 6 minutes was 68.5%, and CO 2 The in-situ conversion rate was 65.1%.
[0036] Example 3 1 g of magnesium carbonate powder was mixed with 100 mg of red mud and added to a glass tube reactor. H2 :O 2 :CO 2 =700:120:200 ml / min of hydrogen-rich gas mixture, ignited at the gas inlet, and the carbonate reaction temperature was controlled at 400 by adjusting the gas flow rate and the height of the solid reactant raw material bed from the flame. o C. After running for 6 minutes, the solids were collected for thermogravimetric analysis of carbonate content, and the gas products entered the mass spectrometer for gas composition and concentration analysis. The results showed that the decomposition rate of magnesium carbonate within 6 minutes was 89.5%, and CO 2 The in situ conversion rate was 55.0%.
[0037] The above examples show that carbonates can be decomposed more quickly when mixed with iron-containing catalysts (solid waste or iron-based catalysts) and combusted in a high-temperature gas stream containing a hydrogen-rich mixed gas, while the released carbon dioxide can be converted in situ.
[0038] Application Examples This application example provides a method for zero-carbon decomposition of carbonate hydrogenation reduction based on self-heating of hydrogen combustion. Figure 1 The system shown.
[0039] like Figure 1 As shown, the reactor in the system includes: a reactor body 1, a feed port 2, a discharge port 3, a mixed gas inlet 4 (with a burner), a calcined gas product outlet 5, and a CO 2 Circulation pipeline 6. Among them, the solid raw material is a powder mixture of carbonate raw material F1 and iron-containing solid waste F2, which enters the reactor body 1 from the feed port 2 at the top of the reactor. The mixed gas F4 enters the reactor body 1 from the mixed gas inlet 4 at the bottom of the side and burns, generating high-temperature hydrogen-rich gas to participate in the gas-solid reaction in the reactor. The solid powder flow and the flue gas flow move in opposite directions, and the metal oxide product F3 obtained by decomposition gradually descends to the discharge port 3 at the bottom under the action of gravity and moves out of the reactor; while the reaction gas product F5 is discharged from the calcined gas product outlet 5 on the top side. Furthermore, the pipeline connected to the calcined gas product outlet 5 is provided with a gas separator, and the separated CO 2 By CO 2 The circulating pipe 6 is mixed with the raw gas hydrogen and oxygen in proportion and enters the reactor for subsequent reaction.
[0040] This application example provides a method for zero-carbon decomposition of carbonate by hydrogenation reduction based on self-heating of hydrogen combustion, comprising the following steps: Step 1: adding the iron-containing solid waste F2 and the carbonate raw material F1 to the decomposition furnace reactor body 1 from the feed port 2 at the same time; controlling the mass ratio of the iron-containing solid waste F2 to the carbonate raw material F1 to be 1: (5-20); The carbonate raw materials include one or more of calcium carbonate, magnesium carbonate, ferrous carbonate, limestone, dolomite, marble, calcite, magnesite, and siderite; the iron-containing solid waste includes one or more of red mud, steel slag, fly ash, coal gangue, iron ore powder, etc. Adding cheap iron-containing solid waste as a catalyst to the carbonate raw materials can achieve carbonate hydrogenation catalytic decomposition and CO at a lower temperature. 2 In-situ conversion has significant benefits in energy saving and emission reduction.
[0041] Step 2: Hydrogen, oxygen and carbon dioxide are mixed in a volume ratio of (6-8): (1-1.5): (0.5-3), and the mixed gas enters the reactor body 1 through the mixed gas inlet 4 and burns, generating hydrogen flame combustion and a high-temperature hydrogen-rich atmosphere; the hydrogen is prepared using renewable energy (such as wind, light and other renewable energy).
[0042] Step 3: Under the catalytic action of iron-containing solid waste, the pyrolysis of carbonate is achieved by using the self-heating of hydrogen combustion. The pyrolysis temperature of carbonate is 600-1260°C, and the carbon dioxide generated by the pyrolysis of carbonate is converted in situ by using hydrogen. The high-temperature mixed gas flows upward from the burner, and the carbonate solid raw material doped with the iron-containing solid waste catalyst flows downward from the top feed port 2. The two flow in opposite directions, and the high-temperature mixed gas interacts with the carbonate, and a reaction of carbonate pyrolysis coupled with hydrogen molecule catalytic reduction occurs. After a certain reaction time, metal oxide product F3 and reaction gas product F5 are obtained; The flow rate of the mixed gas is controlled to be 9-10 m / s, and the feeding rate of the mixed system of the iron-containing catalyst and the carbonate raw material is 1000-1500 t / d. Under this condition, the residence time of the solid raw material in the reactor area is 10-20s, so that the powder raw material particles are decomposed in a suspended state in the reactor.
[0043] Step 4: The metal oxide product F3 gradually descends to the discharge port 3 at the bottom under the action of gravity and moves out of the reactor, while the reaction gas product F5 is discharged from the calcination gas product outlet 5 on the top side.
[0044] Step 5: Separate and collect the carbon dioxide in the reaction gas product F5. 2 F8 by CO 2 The circulating pipeline 6 is mixed with hydrogen F6 and oxygen F7 to form a mixed gas F4, which enters the reactor again for subsequent reactions.
[0045] In summary, the system and method provided by the present invention can achieve dual carbon reduction benefits at the heating end and the carbonate decomposition end by using green hydrogen to replace traditional coal. Among them, the use of hydrogen combustion to provide energy can produce clean water vapor products, and the excess high-temperature hydrogen reacts with carbonate doped with iron-containing solid waste to undergo catalytic hydrogenation reaction, which can effectively reduce the carbonate decomposition temperature and energy consumption, and at the same time achieve the CO reduction in the carbonate decomposition process. 2 The in-situ conversion and utilization of carbonates can ultimately achieve zero-carbon decomposition of carbonates, thereby reducing the economic cost of the production process.
[0046] The above are only preferred embodiments of the present invention, and are not intended to limit the implementation methods and protection scope of the present invention. Those skilled in the art should be aware that all solutions obtained by equivalent substitutions and obvious changes made using the contents of the specification of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for zero-carbon decomposition of carbonate by hydrogenation reduction based on self-heating of hydrogen combustion, It is characterized in that The following steps are involved: A mixed gas is formed by mixing hydrogen, oxygen and carbon dioxide in a volume ratio of (6-8): (1-1.5): (0.5-3); the mixed gas is introduced into a mixed system of a carbonate raw material and an iron-containing catalyst; under the catalytic action of the iron-containing catalyst, the carbonate is pyrolyzed by self-heating by combustion of part of the hydrogen, and the carbon dioxide generated by the pyrolysis of the carbonate is converted in situ by using the unburned hydrogen.
2. The method according to claim 1, It is characterized in that The hydrogen is prepared by using renewable energy.
3. The method according to claim 1, It is characterized in that The carbonate raw material includes one or more combinations of calcium carbonate, magnesium carbonate, ferrous carbonate, limestone, dolomite, marble, calcite, magnesite, and siderite.
4. The method according to claim 1, It is characterized in that The iron-containing catalyst comprises one or more combinations of iron-containing solid waste, active iron species extracted from the iron-containing solid waste, and catalysts modified with the iron-containing solid waste as a matrix.
5. The method according to claim 1, It is characterized in that The mass ratio of the iron-containing catalyst to the carbonate raw material is 1:(5-20).
6. The method according to claim 1, It is characterized in that The carbon dioxide in the mixed gas includes the carbon dioxide that is not reacted in the in-situ conversion.
7. The method according to claim 1, It is characterized in that The ratio of the flow rate of the mixed gas to the feed mass of the mixing system per unit time is 1: (5-7) L / g.
8. The method according to claim 7, It is characterized in that The flow rate of the mixed gas is 1-5 L / min; the feeding rate of the mixed system is 0.1-0.5 g / s.
9. The method according to claim 1, It is characterized in that The pyrolysis temperature of the carbonate is 600-1260°C.
10. A system for carbonate hydrogenation reduction zero-carbon decomposition based on hydrogen combustion self-heating according to any one of claims 1 to 9, It is characterized in that The system comprises: a reactor body (1), a feed inlet (2), a discharge port (3), a mixed gas inlet (4), a calcined gas product outlet (5), and a CO 2 Circulation pipe (6).
Citation Information
Cited By
Low-carbon cement production method for co-producing high-value chemicals