Preparation method and application of amorphous MoS5 + x magnesium ion battery positive electrode material

By preparing amorphous MoS5+x positive electrode material, the problems of lithium-ion batteries in high-speed discharge and safety are solved, the performance of magnesium ion batteries is improved, high energy density and excellent cycle life are achieved, and suitable for large-scale power grids Energy storage and electric vehicles.

CN118908278AActive Publication Date: 2024-11-08YANTAI UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411073354.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-08
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

Lithium-ion batteries have poor power density during high-rate discharge, which has the risk of thermal runaway and high cost. The performance of the cathode material of magnesium-ion batteries is poor, resulting in challenges in rapid energy release and safety.

Method used

Molybdenum polysulfide is prepared by using the preparation method of amorphous MoS5+x positive electrode material. By using molybdate, reducing agent and ammonium polysulfide as reaction raw materials, it is stirred, washed and vacuum oven-dried to prepare molybdenum polysulfide for the positive electrode material of magnesium ion battery , improve its electrochemical properties.

Benefits of technology

It realizes the high energy density and excellent cycle life of magnesium ion batteries, improves its application prospects in large-scale grid energy storage, electric vehicles and portable equipment, and provides safer and more efficient energy solutions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908278A_ABST
    Figure CN118908278A_ABST
Patent Text Reader

Abstract

The invention relates to the field of battery materials, and discloses a preparation method and application of an amorphous MoS5 + x positive electrode material, firstly, ammonium polythiomolybdate is prepared by adopting molybdate, a reducing agent and a certain amount of ammonium polysulfide as reaction raw materials, the ammonium polythiomolybdate is dissolved in deionized water and stirred, oxalic acid is dropwise added into the solution, stirring continues to be carried out, and the amorphous MoS5 + x positive electrode material is obtained. And washing and centrifuging, drying in a vacuum oven to obtain molybdenum polysulfide (MoS5 + x), storing in a dryer, and using the molybdenum polysulfide as the positive electrode material of the magnesium ion battery. The amorphous MoS5 + x positive electrode material is excellent in electrochemical performance, and the ultrahigh reversible capacity, the excellent coulombic efficiency and the lasting cycle life of the amorphous MoS5 + x positive electrode material exceed those of a current mainstream magnesium ion battery positive electrode material. The obvious magnesium storage performance endows the amorphous MoS5 + x positive electrode material with application prospects in magnesium ion batteries and other electrochemical energy storage equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery materials, in particular to amorphous MoS 5+x Preparation method and application of positive electrode materials. Background Art

[0002] Lithium-ion batteries have many well-known advantages, such as high energy density, mature manufacturing processes and a wide range of applications. However, the above advantages do not cover up some of their performance defects. For example, the power density of lithium-ion batteries is poor at high discharge rates, which limits their performance in applications that require rapid energy release. In addition, due to the risk of thermal runaway, which may cause the battery to overheat and even cause fire or explosion, its safety issues have always been a concern. At the same time, due to the limited lithium resources, the cost of lithium-ion batteries has remained high, which to some extent hinders its application in large-scale energy storage.

[0003] In contrast, magnesium-ion batteries (MIBs) are regarded as a promising electrochemical energy storage technology due to their unique advantages. First, magnesium is abundant and inexpensive, which gives magnesium-ion batteries a clear cost advantage. Secondly, the environmental friendliness of magnesium-ion batteries is also an important reason for their attention, which is in line with the current pursuit of green and sustainable energy. Most importantly, compared with lithium metal electrodes, magnesium electrodes have almost no tendency to form dendrites, the formation of which can cause battery short circuits and lead to safety problems. Therefore, magnesium-ion batteries have significant advantages in safety.

[0004] These advantages make magnesium-ion batteries a promising electrochemical energy storage device, which may replace traditional lithium-ion batteries in the future and provide safer, more efficient and environmentally friendly energy solutions for large-scale grid energy storage, electric vehicles and portable electronic devices. However, the poor performance of the cathode material is the current weakness of MIBs. Therefore, it is urgent to develop new cathode materials to promote their development. The main reason for the poor performance of MIBs cathode comes from Mg 2+ Ion. Mg 2+ Bili + small, has two positive charges, resulting in Mg 2+ It has a strong interaction with the positive electrode and is difficult to embed into the positive electrode lattice, causing its diffusion kinetics to deteriorate. In addition, due to the crystalline structure, Mg 2+ The reaction energy barrier of crystalline positive electrode materials is significantly enhanced. Compared with crystalline materials, amorphous materials can provide three-dimensional diffusion channels, and the diffusion energy barrier can be effectively reduced, thereby improving the magnesium storage capacity. Compared with MoS2, molybdenum polysulfide has polysulfur characteristics, which not only contains S 2-, and also includes S2 2- , anions and cations can undergo redox reactions simultaneously, providing a higher magnesium storage capacity, and are very promising positive electrode materials for rechargeable magnesium ion batteries. Therefore, amorphous molybdenum polysulfide is considered to be an ideal choice for high-performance rechargeable magnesium ion battery positive electrode materials.

[0005] To this end, the present invention proposes amorphous MoS 5+x The invention relates to a preparation method and application of a positive electrode material for a magnesium ion battery, so as to optimize the performance of the magnesium ion battery and obtain a positive electrode material for a magnesium ion battery with a high energy density. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention provides an amorphous MoS 5+x The preparation method of positive electrode materials can not only improve the performance of magnesium-ion batteries, but also provide strong technical support for their applications in large-scale grid energy storage, electric vehicles, and portable electronic devices.

[0007] To achieve the above objectives, the present invention is implemented by the following technical solutions: amorphous MoS 5+x The method for preparing a positive electrode material comprises the following steps:

[0008] S1: using molybdate, a reducing agent and a certain amount of ammonium polysulfide as reaction raw materials to prepare ammonium polysulfide molybdate;

[0009] S2: Dissolve ammonium polysulfide molybdate in deionized water, stir, then add oxalic acid dropwise to the solution, continue stirring, wash and centrifuge, and dry in a vacuum oven to obtain molybdenum polysulfide (MoS 5+x ), stored in a desiccator;

[0010] Preferably, in step S1, the reducing agent includes but is not limited to hydroxylamine hydrochloride, hydrazine hydrate, and sodium borohydride.

[0011] Preferably, in step S2, the types of the acid include but are not limited to oxalic acid, hydrochloric acid, and glacial acetic acid.

[0012] Preferably, a magnesium ion battery, wherein the positive electrode of the magnesium ion battery is composed of amorphous MoS 5+x Positive electrode material composition.

[0013] Preferably, the negative electrode of the magnesium ion battery includes but is not limited to magnesium metal and magnesium alloy.

[0014] Preferably, the electrolyte of the battery is an electrolyte suitable for magnesium ion batteries, including but not limited to (PhMgCl)2-AlCl3 / THF electrolyte, Mg(TFSI)2-MgCl2 electrolyte, and (R-PhOMgCl)2-AlCl3 / THF electrolyte.

[0015] Preferably, the battery is at 0.1Ag -1 At a current density of 1.5 %, after 90 charge and discharge cycles, it can provide 685 mAh g -1 The reversible capacity of the battery is ≥95% and the coulombic efficiency of the battery during charge and discharge is ≥95% at 1Ag -1 At a rate of 200 mAh g -1 above.

[0016] The present invention provides amorphous MoS 5+x The preparation method and application of positive electrode materials have the following beneficial effects:

[0017] 1. Amorphous MoS of the present invention 5+x The cathode material has excellent electrochemical performance. Its high reversible capacity, superior coulombic efficiency and long cycle life all surpass the current mainstream magnesium ion battery cathode materials. The optimization of this performance makes amorphous MoS 5+x Positive electrode materials have broad application prospects in high-performance magnesium-ion batteries and other energy storage devices.

[0018] 2. The preparation method of the present invention adopts the strategy of adding acid and stirring after synthesizing the precursor at low temperature, and the operation process is simple and the reaction conditions are easy to control. This feature enables the method to be easily implemented in large-scale production, further improving production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The MoS obtained in Example 1 5+x TEM image of positive electrode material; TEM image of MoS3 positive electrode material prepared in comparative example 1; TEM image of MoS2 positive electrode material prepared in comparative example 2.

[0020] Figure 2 The MoS obtained in Example 1 5+x XRD spectrum of positive electrode material; XRD spectrum of MoS3 positive electrode material prepared in comparative example 1; XRD spectrum of MoS2 positive electrode material prepared in comparative example 2.

[0021] Figure 3 The MoS obtained in Example 1 5+x Raman spectrum of positive electrode material; Raman spectrum of MoS3 positive electrode material prepared in comparative example 1; Raman spectrum of MoS2 positive electrode material prepared in comparative example 2.

[0022] Figure 4 The MoS obtained in Example 1 5+x EDS spectrum of the positive electrode material.

[0023] Figure 5 The MoS obtained in Example 1 5+xThe full battery assembled with positive electrode material, MoS3 positive electrode material obtained in comparative example 1 and MoS2 positive electrode material obtained in comparative example 2 and metal magnesium has a 0.1Ag -1 Cycle performance diagram.

[0024] Figure 6 The MoS obtained in Example 1 5+x Rate performance diagram of a full battery assembled with the positive electrode material, the MoS3 positive electrode material obtained in Comparative Example 1, and the MoS2 positive electrode material obtained in Comparative Example 2 and metallic magnesium. DETAILED DESCRIPTION

[0025] The following will be combined with the drawings in the specification of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Example:

[0027] Please see attached Figure 1 -Attached Figure 6 :

[0028] Embodiment 1:

[0029] First, weigh 8.0g of ammonium molybdate tetrahydrate and 6.0g of hydroxylamine hydrochloride and dissolve them in 120mL of deionized water, stir and mix with 120mL of ammonium polysulfide solution to obtain a mixed solution. Then, the mixed solution was placed in a 50°C oven for 1 hour, washed and centrifuged after standing for 1 hour to obtain a filtrate. The filtrate was placed in a 90°C oven for 4 hours, washed and centrifuged after standing for 1 hour. Next, 40mL of ammonium polysulfide was dropped into the filtrate, stirred vigorously, and stood for 12 hours. After that, the ammonium dodecylthiomolybdate raw material was collected by filtration, and the black crystals were further washed twice with 30mL of ice water, isopropanol, carbon disulfide, and ether. The black crystals were then dried in a vacuum oven at room temperature and then stored in a dryer. Finally, 0.15g of ammonium dodecylthiomolybdate was dissolved in 50mL of secondary water, 12.5mL of 1M oxalic acid was added dropwise to the above solution, stirred for 2 hours, and centrifuged to prepare amorphous MoS 5+x Material.

[0030] Embodiment 2:

[0031] First, weigh 8.0g of ammonium molybdate tetrahydrate and 6.0g of hydroxylamine hydrochloride and dissolve them in 120mL of deionized water, stir and mix with 120mL of ammonium polysulfide solution to obtain a mixed solution. Then, the mixed solution was placed in a 50°C oven for 1 hour, washed and centrifuged after standing for 1 hour to obtain a filtrate. The filtrate was placed in a 90°C oven for 4 hours, washed and centrifuged after standing for 1 hour. Next, 40mL of ammonium polysulfide was dropped into the filtrate, stirred vigorously, and stood for 12 hours. After that, the ammonium dodecylthiomolybdate raw material was collected by filtration, and the black crystals were further washed with 30mL of ice water, isopropanol, carbon disulfide, and ether twice each. The black crystals were then dried in a vacuum oven at room temperature and then stored in a dryer. Finally, 0.15g of ammonium dodecylthiomolybdate was dissolved in 50mL of secondary water, 12.5mL of 1M glacial acetic acid was added dropwise to the above solution, stirred for 2 hours, and centrifuged to prepare amorphous MoS 5+x Material.

[0032] Embodiment 3:

[0033] First, 8.0g of ammonium molybdate tetrahydrate and 4.32g of hydrazine hydrate were weighed and dissolved in 120mL of deionized water, stirred and mixed with 120mL of ammonium polysulfide solution to obtain a mixed solution. Then, the mixed solution was placed in a 50°C oven for 1 hour, washed and centrifuged after standing for 1 hour to obtain a filtrate. The filtrate was placed in a 90°C oven for 4 hours, washed and centrifuged after standing for 1 hour. Next, 40mL of ammonium polysulfide was dropped into the filtrate, stirred vigorously, and stood for 12 hours. After that, the ammonium dodecyl sulfide molybdate raw material was collected by filtration, and the black crystals were further washed twice with 30mL of ice water, isopropanol, carbon disulfide, and ether. The black crystals were then dried in a vacuum oven at room temperature and then stored in a dryer. Finally, 0.15g of ammonium dodecyl thiomolybdate was dissolved in 50mL of secondary water, 12.5mL of 1M oxalic acid was added dropwise to the above solution, stirred for 2 hours, and centrifuged to prepare amorphous MoS 5+x Material.

[0034] Summary: The above three examples describe in detail the method of successfully preparing MoS5 positive electrode materials using different reducing agents and acids. These examples show that the preparation method of the present invention has the advantages of simple operation, mild reaction conditions, high product purity, high yield, etc., and can effectively prepare amorphous MoS with excellent electrochemical properties. 5+x Positive electrode material, suitable for energy storage fields such as magnesium ion batteries.

[0035] Comparative Example 1:

[0036] 7g of ammonium molybdate tetrahydrate, 30mL of water and ammonia water were placed in a 500mL flask, stirred in an oil bath at 70℃ for 60min, and then 550mL of ammonium sulfide solution was added. The solution was stirred in an oil bath at 70℃ for 2h. The solution turned red, cooled, and filtered with isopropanol and ether to obtain (NH4)2MoS 4, 70 mL of (NH4)2MoS4 was added to 20 mL of deionized water and stirred for 1 hour. HCl was added dropwise into the above solution to make the pH equal to 3. The solution was stirred for 2 hours and centrifuged to prepare an amorphous MoS3 positive electrode material.

[0037] Comparative Example 2:

[0038] 60 mg of ammonium molybdate tetrahydrate was added to 50 mL of deionized water. After ultrasonication for 5 minutes, 1.7 mL of hydrazine hydrate was added to the above solution and stirred for 20 minutes. The dark red solution was then quickly transferred to a 50 mL reactor and reacted in an oven at 150 ° C for 6 hours. Finally, the amorphous MoS2 positive electrode material was prepared by washing with water and ethanol 5 times.

[0039] The positive electrode materials obtained in Examples 1-3 and Comparative Example 1 were mixed with acetylene black and PVDF in a weight ratio of 7:2:1 to form a slurry. The slurry was evenly applied on a copper foil, and the electrode sheets were cut and pressed. Finally, the electrode sheets were vacuum dried at 60°C for 6 hours to obtain the electrode sheets. The electrode sheets were directly used as the positive electrode, the magnesium sheet was used as the negative electrode, the organic electrolyte was (PhMgCl)2-AlCl3 / THF electrolyte containing 1-butyl-1-methylpyridinium chloride ([BMP]Cl), and button batteries were assembled.

[0040] Figure 1 The MoS obtained in Example 1 5+x TEM images of positive electrode materials (a), (b), TEM images of MoS3 positive electrode materials obtained in comparative example 1 (c), (d), and TEM images of MoS2 positive electrode materials obtained in comparative example 2 (e), (f). The materials in a and b are nanoparticles with uniform morphology, and the diameter of the nanoparticles is about 12 to 58 nm. The materials in c and d are also nanoparticles with uniform morphology, and the diameter of the nanoparticles is about 12 to 52 nm, which are of comparable size. The materials in e and f are nanospheres assembled from nanosheets with uniform morphology, and the average size of the nanospheres is 80 to 100 nm.

[0041] Figure 2 The MoS obtained in Example 1 5+x The XRD spectrum of the positive electrode material, the XRD spectrum of the MoS3 positive electrode material obtained in Comparative Example 1, and the XRD spectrum of the MoS2 positive electrode material obtained in Comparative Example 2 show that MoS 5+x , MoS3 and MoS2 are all amorphous.

[0042] Figure 3The MoS obtained in Example 1 5+x The Raman spectrum of the positive electrode material, the Raman spectrum of the MoS3 positive electrode material obtained in Comparative Example 1, and the Raman spectrum of the MoS2 positive electrode material obtained in Comparative Example 2 show that the amorphous MoS 5+x 130 to 250 cm in Raman images -1 The Raman peaks are attributed to Mo-Mo stretching vibration, 250 to 400 cm -1 The Raman peak of amorphous MoS3 is attributed to Mo-S stretching vibration. -1 and 347cm -1 The two Raman peaks are attributed to the Mo-S stretching vibration in MoS3. The Raman vibration peak of amorphous MoS2 is different, located at 140 cm -1 , 188cm -1 and 339cm -1 Corresponding to the J1, J2 and J3 modes of the metallic 1T phase, the other three are located at 275.7 cm -1 、370cm -1 and 400cm -1 The three peaks correspond to the E1g, E2g and A1g vibration modes of the semiconductor 2H phase.

[0043] Figure 4 The MoS obtained in Example 1 5+x EDS spectrum of the positive electrode material. From the EDS spectrum results, it can be seen that the molybdenum-sulfur molar ratio of the positive electrode material is 1:5.7, confirming the polysulfur-rich MoS 5+x Successful preparation.

[0044] Figure 5 The MoS obtained in Example 1 5+x The button cell assembled with positive electrode material, MoS3 positive electrode material obtained in comparative example 1 and MoS2 positive electrode material obtained in comparative example 2 and metal magnesium was tested at 0.1Ag. -1 Cyclic performance diagram of current density, after 90 cycles of Mg 2+ Insertion / extraction, MoS obtained in Example 1 5+x The positive electrode material can still provide 685mAh g -1 The ultra-high reversible capacity is significantly higher than the 350 mAh g provided by the MoS3 cathode material in Comparative Example 1. -1 The MoS2 positive electrode material of Comparative Example 2 provided 239 mAh g -1 , indicating that the increase in the number of sulfur ions plays a key positive role in improving the magnesium storage capacity.

[0045] Figure 6 The MoS obtained in Example 1 5+xThe button cells assembled with the MoS3 positive electrode material obtained in the positive electrode material and the metal magnesium in the comparative example 1 were subjected to 90 cycles of rate performance test at different current densities. 5+x Has the best rate performance (even at 1A g -1 The specific capacity is still 200 mAh g -1 The results are as follows (above), which are significantly better than the MoS3 prepared in Comparative Example 1 and the MoS2 prepared in Comparative Example 2.

[0046] Although embodiments of the present invention have been described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. Amorphous MoS 5+x A method for preparing a positive electrode material, characterized in that: The following steps are involved: S1: using molybdate, a reducing agent and a certain amount of ammonium polysulfide as reaction raw materials to prepare ammonium polysulfide molybdate; S2: Dissolve ammonium polysulfide molybdate in deionized water, stir, then add oxalic acid dropwise to the solution, continue stirring, wash and centrifuge, and dry in a vacuum oven to obtain molybdenum polysulfide (MoS 5+x ), store in a desiccator.

2. Amorphous MoS according to claim 1 5+x A method for preparing a positive electrode material, characterized in that: In the step S1, the reducing agent includes but is not limited to hydroxylamine hydrochloride, hydrazine hydrate, and sodium borohydride.

3. Amorphous MoS according to claim 1 5+x A method for preparing a positive electrode material, characterized in that: In the step S2, the stirring time after the oxalic acid is added to the ammonium polythiomolybdate solution is 1.5 hours to 2 hours.

4. The amorphous MoS according to claim 1 5+x A method for preparing a positive electrode material, characterized in that: In the step S2, the types of the acid include but are not limited to oxalic acid, hydrochloric acid, and glacial acetic acid.

5. A magnesium ion battery, characterized in that: The positive electrode of the magnesium ion battery is prepared by the amorphous MoS 5+x Positive electrode material composition.

6. A magnesium ion battery according to claim 5, characterized in that: The negative electrode of the magnesium ion battery includes but is not limited to magnesium metal and magnesium alloy.

7. A magnesium ion battery according to claim 5, characterized in that: The electrolyte of the battery is an electrolyte suitable for magnesium ion batteries, including but not limited to (PhMgCl)2-AlCl3 / THF electrolyte, Mg(TFSI)2-MgCl2 electrolyte, and (R-PhOMgCl)2-AlCl3 / THF electrolyte.

8. A magnesium ion battery according to claim 6, characterized in that: The battery is at 0.1Ag -1 At a current density of 1.5 %, after 90 charge and discharge cycles, it can provide 685 mAh g -1 The high reversible capacity and the coulombic efficiency of the charge and discharge process are ≥95% at 1Ag -1 At a rate of 200 mAh g -1 above.

Citation Information

Patent Citations

  • Hollow carbon sphere loaded MoS3 magnesium ion battery positive electrode material and preparation method thereof

    CN118231628A

  • Magnesium ion battery and preparation method therefor

    WO2017206063A1