Battery positive electrode material giving consideration to both first efficiency and cycle performance and preparation method of battery positive electrode material
By covering Li5FeO4 on the outer surface of the lithium manganate positive electrode material, the problem of poor circulation performance is solved, and the performance of lithium-ion batteries with high efficiency and long life is achieved, especially the stability improvement at high voltages.
Patent Information
- Application Number
- CN202410883682.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-11-08
AI Technical Summary
The lithium manganate positive electrode material has a ginger-Taylor effect and the dissolution effect of Mn3+ ions during the circulation process, resulting in poor circulation and self-discharge performance, which limits its promotion in high-performance applications.
The positive electrode material is prepared by coating Li5FeO4 on the outer surface of LiMn2O4 and using disperser mixing, vacuum drying and grinding to form a composite material with lithium-rich ferrate coated lithium manganate to reduce the Jahn-Teller effect and improve electrochemistry Interface stability.
It effectively improves the first-time efficiency and circulation performance of the positive electrode material, extends the service life of the battery, and maintains good circulation performance at high voltages of 4.2-4.4V.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a battery positive electrode material having both initial efficiency and cycle performance and a preparation method thereof. Background Art
[0002] As the most promising energy storage power source, lithium-ion batteries are widely used in consumer electronics, transportation, and energy storage systems. Their performance largely determines the performance and reliability of these applications. In lithium-ion batteries, the cathode material is the main site for the reversible insertion and extraction of lithium ions, which has an important impact on the capacity, cycle life, and safety of the battery. Therefore, researching and developing high-performance cathode materials has become the key to improving the overall performance of lithium-ion batteries.
[0003] At present, the positive electrode materials of lithium-ion batteries mainly include lithium cobalt oxide (LiCoO2), nickel cobalt manganese oxide (NCM), lithium iron phosphate (LiFePO4) and lithium manganese oxide (LiMn2O4). Among them, lithium manganese oxide has attracted widespread attention due to its low raw material cost and high safety performance. However, the mass specific capacity of lithium manganese oxide is relatively low, and there is the Jahn-Teller Effect and the dissolution effect of trivalent Mn ions during the cycle process, resulting in poor cycle performance and self-discharge performance, which limits its promotion in high-performance applications.
[0004] The Chiang-Taylor effect can cause the crystal structure of lithium manganese oxide to be distorted, leading to the degradation of electrochemical performance, especially in high-rate charge and discharge cycles. 3+ The dissolution effect of ions will lead to the loss of manganese elements and electrolyte contamination, further reducing the cycle stability and initial charge and discharge efficiency of the battery. Therefore, how to improve the initial efficiency and cycle performance of lithium manganese oxide positive electrode materials through material modification has become an urgent problem to be solved.
[0005] In view of this, it is indeed necessary to modify the existing lithium manganese oxide materials to improve both their initial efficiency and cycle performance, which is of great significance for further improving the overall performance of lithium-ion batteries and meeting the growing demand for high-performance energy storage. Summary of the invention
[0006] The object of the present invention is to provide a method for preparing a positive electrode material for a battery that takes both initial efficiency and cycle performance into consideration, and the prepared positive electrode material can simultaneously improve the cycle performance and initial efficiency of the battery.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] A method for preparing a positive electrode material for a battery that takes both initial efficiency and cycle performance into consideration, the positive electrode material comprising LiMn2O4 and Li5FeO4 coated on the outer surface of the LiMn2O4;
[0009] The method for preparing the positive electrode material comprises the following steps:
[0010] Preparation of Li5FeO4:
[0011] 1) weighing and mixing LiOH·H2O and Fe(NO3)3·9H2O at a molar ratio of Li:Fe of 8:1 to obtain a mixed material;
[0012] 2) Drying the mixed material;
[0013] 3) Grind the mixed material and pre-sinter at a temperature of 400-600°C for 6-10 hours;
[0014] 4) Grind and roast the mixed materials at a temperature of 800-1000°C for 8-20 hours;
[0015] 5) grinding the product obtained in step 4) to obtain Li5FeO4;
[0016] Preparation of positive electrode materials:
[0017] a) mixing LiMn2O4 and Li5FeO4 in a mass ratio of 99:1 to 90:10;
[0018] b) adding a dispersant, mixing evenly with a disperser, vacuum drying at 150-300° C. for 2-4 hours, and grinding to control the particle size to 10-90 nm, thereby obtaining a positive electrode composite material.
[0019] Preferably, the method further comprises the step of preparing LiMn2O4: weighing, mixing and sintering MnO2 and a lithium source according to a molar ratio of Mn:Li of 2:1.05 to obtain LiMn2O4.
[0020] Preferably, the method further comprises the step of preparing LiMn2O4: weighing, mixing and sintering Mn3O4 and a lithium source according to a molar ratio of Mn:Li of 2:1.05 to obtain LiMn2O4.
[0021] Preferably, in step 2) of preparing Li5FeO4, the drying temperature is 80-150°C and the time is 2-4h.
[0022] Preferably, in step b) of preparing the positive electrode material, the dispersant is at least one of isopropanol and ethanol.
[0023] Preferably, the preparation of the positive electrode material further comprises step c):
[0024] The positive electrode composite material powder is added to the silk protein modified carbon nanotube solution, the mass ratio of the positive electrode composite material powder to the silk protein modified carbon nanotube solution is 1: (1.8-2), the mixture is stirred evenly to obtain a composite solution, and the composite solution is vacuum filtered to obtain a composite material uniformly coated with the silk protein modified carbon nanotubes;
[0025] Dry the filter cake at 80-90°C for 1-2 hours to remove surface moisture; freeze-dry the dried material using a liquid nitrogen freeze dryer to ensure that the moisture inside the material is completely removed and its structural integrity is maintained;
[0026] The dried material is further dried at 140-150° C. for 1-2 hours to obtain a modified positive electrode composite material.
[0027] Preferably, the preparation method of the silk protein modified carbon nanotube solution is:
[0028] Adding multi-walled carbon nanotubes to deionized water, with a mass ratio of multi-walled carbon nanotubes to deionized water being 5:100, and ultrasonically treating for 30 to 40 minutes to obtain a uniformly dispersed carbon nanotube solution;
[0029] Dissolve silk protein in deionized water, stir evenly, and prepare a silk protein solution with a mass concentration of 1%;
[0030] The carbon nanotube solution is slowly added into the silk protein solution, and the mixture is continuously stirred and ultrasonically treated for 15 to 20 minutes to obtain a silk protein modified carbon nanotube solution.
[0031] Preferably, the preparation of the positive electrode material further comprises step d):
[0032] The positive electrode composite material powder is uniformly mixed with the surfactant solution and the template solution, wherein the mass ratio of the positive electrode composite material, the surfactant solution and the template solution is 1.25:1:1, and the composite material having a nanostructure is self-assembled at 60° C. under stirring conditions;
[0033] The self-assembled composite material was immersed in HF solution and stirred for 2 to 4 hours to ensure that the template was completely removed and the nanostructure was retained, and then filtered and washed with deionized water for multiple times to remove the residual HF;
[0034] The filter cake is dried at 80°C for 2-3 hours to remove surface moisture; and then further dried at 150°C-300°C for 2-3 hours to obtain a positive electrode composite material with a nanostructure.
[0035] Preferably, the surfactant solution is a surfactant solution having a mass concentration of 2% formed by uniformly dispersing sodium dodecyl sulfate in deionized water;
[0036] The template solution is a template solution with a mass concentration of 2% formed by uniformly dispersing SiO2 nanospheres in deionized water.
[0037] In addition, the present invention also provides a battery positive electrode material that takes both initial efficiency and cycle performance into consideration, which is prepared by the preparation method of the battery positive electrode material that takes both initial efficiency and cycle performance into consideration as described in any of the above paragraphs.
[0038] In addition, the present invention also provides a lithium ion battery positive electrode, which includes the above-mentioned battery positive electrode material that takes both initial efficiency and cycle performance into consideration.
[0039] In addition, the present invention also provides a lithium ion battery, which includes the above-mentioned lithium ion battery positive electrode.
[0040] Preferably, the negative electrode of the lithium-ion battery adopts a silicon-carbon negative electrode.
[0041] The beneficial effects of the present invention are as follows: the present invention provides a method for preparing a positive electrode material for a battery that takes into account both initial efficiency and cycle performance. The positive electrode material can effectively improve the initial efficiency and cycle performance of the positive electrode material by coating Li5FeO4 on the surface of LiMn2O4; Li5FeO4 is a lithium-rich material. After the battery is formed, its decomposition can generate LFP, forming a stable electrochemical interface, reducing the surface reaction of LiMn2O4, thereby improving the cycle stability. In addition, the battery made using the positive electrode material of the present invention can operate at a higher voltage of 4.2-4.4V and show improved cycle performance, which helps to improve the energy density and service life of the battery. DETAILED DESCRIPTION
[0042] In order to make the technical solutions and advantages of the present invention clearer, the technical solutions of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] According to a first aspect of the present invention, the present invention discloses a method for preparing a positive electrode material for a battery that takes into account both initial efficiency and cycle performance, the positive electrode material comprising LiMn2O4 and Li5FeO4 coated on the outer surface of the LiMn2O4;
[0044] The method for preparing the positive electrode material comprises the following steps:
[0045] Preparation of Li5FeO4:
[0046] 1) weighing and mixing LiOH·H2O and Fe(NO3)3·9H2O at a molar ratio of Li:Fe of 8:1 to obtain a mixed material;
[0047] 2) Drying the mixed material;
[0048] 3) Grind the mixed material and pre-sinter at a temperature of 400-600°C for 6-10 hours;
[0049] 4) Grind and roast the mixed materials at a temperature of 800-1000°C for 8-20 hours;
[0050] 5) grinding the product obtained in step 4) to obtain Li5FeO4;
[0051] Preparation of positive electrode materials:
[0052] a) Mix LiMn2O4 and Li5FeO4 in a mass ratio of 99:1 to 90:10, and adjust the conductivity and stability of the material according to actual needs to optimize the overall performance of the battery;
[0053] b) adding a dispersant, mixing evenly with a disperser, vacuum drying at 150-300° C. for 2-4 hours, and grinding to control the particle size to 10-90 nm, thereby obtaining a positive electrode composite material.
[0054] The present invention performs pre-sintering at 400-600° C. and sintering at 800-1000° C., which can effectively control the crystal structure of the material and improve its electrochemical performance.
[0055] Among them, through vacuum drying and grinding, the particle size is controlled at 10 to 90 nm, which helps to increase the specific surface area and electrochemical activity of the material.
[0056] The present invention uses a lithium-rich lithium iron oxide positive electrode lithium supplementation additive to coat the lithium manganese oxide material. In the first formation stage, it is charged to the target voltage (4.2V) to fully remove the lithium in Li5FeO4, and the remaining LiFeO2 is used as a coating agent to coat the surface of LiMn2O4. In this process, the following technical effects can be achieved:
[0057] 1) Lithium manganate material is coated with LFP (3.5V: Li5FeO4→Li3FeO 3.5 +0.25O2(gas)+2Li + +2e - ; 4.0V: Li3FeO 3.5 →LiFeO2+0.75O2(gas)+2Li + +2e - ), reduce the Jahn-Teller effect;
[0058] 2) At the same time, the negative electrode uses Li rich in lithium iron oxide to form a SEI film to improve the initial efficiency of the battery. Therefore, the present invention meets the demand for long-life and high-capacity lithium manganese oxide batteries.
[0059] Therefore, the present invention adopts a positive electrode material formed by lithium-rich ferric acid coated with lithium manganese oxide. After the battery is formed, the lithium-rich ferric acid is decomposed into LFP to form lithium iron phosphate coated lithium manganese oxide, which can effectively improve the cycle performance of lithium manganese oxide and improve the initial efficiency of the battery. In addition, the battery using the positive electrode material of the present invention also has the effect of improving the cycle performance at a higher voltage of 4.2-4.4V.
[0060] In one embodiment of the present invention, the mass ratio of LiMn2O4 to Li5FeO4 is 90:10 or 97:3 or 95:5. This mixing ratio enables the composite material to achieve an optimal balance between conductivity and stability.
[0061] In one implementation of the present application, the step of preparing LiMn2O4 is further included: weighing, mixing and sintering MnO2 and a lithium source according to a molar ratio of Mn:Li of 2:1.05 to obtain LiMn2O4, wherein the lithium source is one of Li2CO3 and LiOH.
[0062] In one implementation of the present application, the step of preparing LiMn2O4 is further included: weighing, mixing and sintering Mn3O4 and a lithium source according to a molar ratio of Mn:Li of 2:1.05 to obtain LiMn2O4, wherein the lithium source is one of Li2CO3 and LiOH.
[0063] In one implementation of the present application, in step 2) of preparing Li5FeO4, the drying temperature is 80-150°C and the time is 2-4h. Drying at 80-150°C ensures that the material reaches an appropriate degree of dryness before grinding and calcining to avoid moisture affecting its performance; and the temperature is controlled at 80-150°C, which helps prevent excessive oxidation and thermal decomposition of the material, thereby maintaining the uniformity and activity of the chemical composition.
[0064] In one implementation of the present application, in step b) of preparing the positive electrode material, the dispersant is at least one of isopropanol and ethanol. Using isopropanol or ethanol as a dispersant helps to optimize the microstructure and electrochemical performance of the material.
[0065] In one implementation of the present application, the preparation of the positive electrode material further includes step c):
[0066] The positive electrode composite material powder is added to the silk protein modified carbon nanotube solution, the mass ratio of the positive electrode composite material powder to the silk protein modified carbon nanotube solution is 1: (1.8-2), the mixture is stirred evenly to obtain a composite solution, and the composite solution is vacuum filtered to obtain a composite material uniformly coated with the silk protein modified carbon nanotubes;
[0067] Dry the filter cake at 80-90°C for 1-2 hours to remove surface moisture; freeze-dry the dried material using a liquid nitrogen freeze dryer to ensure that the moisture inside the material is completely removed and its structural integrity is maintained;
[0068] The dried material is further dried at 140-150° C. for 1-2 hours to obtain a modified positive electrode composite material.
[0069] In one implementation of the present application, the preparation method of the silk protein modified carbon nanotube solution is:
[0070] Adding multi-walled carbon nanotubes to deionized water, with a mass ratio of multi-walled carbon nanotubes to deionized water being 5:100, and ultrasonically treating for 30 to 40 minutes to obtain a uniformly dispersed carbon nanotube solution;
[0071] Dissolve silk protein in deionized water, stir evenly, and prepare a silk protein solution with a mass concentration of 1%;
[0072] The carbon nanotube solution is slowly added into the silk protein solution, and the mixture is continuously stirred and ultrasonically treated for 15 to 20 minutes to obtain a silk protein modified carbon nanotube solution.
[0073] The present invention not only has excellent electrical conductivity, but also good mechanical strength and flexibility by introducing carbon nanotubes modified with silk protein, thereby significantly improving the cycle life and initial efficiency of the battery. In particular, the freeze-drying process ensures the integrity of the internal structure of the material, further improving the stability and conductivity of the material.
[0074] In one implementation of the present application, the preparation of the positive electrode material further includes step d):
[0075] The positive electrode composite material powder is uniformly mixed with the surfactant solution and the template solution, wherein the mass ratio of the positive electrode composite material, the surfactant solution and the template solution is 1.25:1:1, and the composite material having a nanostructure is self-assembled at 60° C. under stirring conditions;
[0076] The self-assembled composite material was immersed in HF solution and stirred for 2 to 4 hours to ensure that the template was completely removed and the nanostructure was retained, and then filtered and washed with deionized water for multiple times to remove the residual HF;
[0077] The filter cake is dried at 80°C for 2-3 hours to remove surface moisture; and then further dried at 150°C-300°C for 2-3 hours to obtain a positive electrode composite material with a nanostructure.
[0078] In one implementation of the present application, the surfactant solution is a surfactant solution having a mass concentration of 2% formed by uniformly dispersing sodium dodecyl sulfate in deionized water;
[0079] The template solution is a template solution with a mass concentration of 2% formed by uniformly dispersing SiO2 nanospheres in deionized water.
[0080] The positive electrode composite material prepared by the self-assembly technology of the present invention has a specific nanostructure, which significantly improves the specific surface area and electrochemical performance of the material; this nanostructure helps to improve the conductivity and ion transmission speed of the electrode material, thereby improving the cycle life and capacity of the battery; in addition, by removing the template and drying treatment, the structural integrity and stability of the material are ensured.
[0081] In one implementation of the present application, the preparation of the positive electrode material further includes step e):
[0082] Dissolving paraffin in ethanol to prepare a paraffin solution with a mass concentration of 5%;
[0083] The positive electrode composite material is immersed in a paraffin solution to ensure complete infiltration, and after being taken out, it is dried at 50° C. for 1 to 2 hours to remove the surface ethanol to obtain a paraffin-coated composite material;
[0084] The coated composite material is dried at 50°C for 2 to 3 hours to ensure that the surface moisture or solvent is completely evaporated; and then further dried at 80°C-100°C for 2 to 3 hours to obtain a modified positive electrode composite material.
[0085] Among them, the uniformity and stability of the coating layer are ensured through staged drying at 50°C and 80-100°C, thereby improving the electrochemical properties of the material.
[0086] The present invention coats the surface of the positive electrode composite material with phase change material paraffin, which can absorb heat and keep the temperature of the battery stable in a high temperature environment, thereby preventing thermal runaway caused by overheating of the battery.
[0087] According to the second aspect of the present invention, the present invention also provides a battery positive electrode material that takes both initial efficiency and cycle performance into consideration, which is prepared by the preparation method of the battery positive electrode material that takes both initial efficiency and cycle performance into consideration as described in any of the above paragraphs.
[0088] According to the third aspect of the present invention, the present invention further provides a lithium-ion battery positive electrode, which comprises the above-mentioned battery positive electrode material that takes both initial efficiency and cycle performance into consideration.
[0089] According to the fourth aspect of the present invention, the present invention also provides a lithium-ion battery, comprising a positive electrode, a separator, an electrolyte and a negative electrode, the positive electrode comprising the positive electrode according to the present invention, specifically, the positive electrode comprising a positive electrode current collector and a positive electrode active material layer, the positive electrode active material layer comprising the positive electrode material according to the present invention.
[0090] positive electrode
[0091] The positive electrode comprises a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector. The positive electrode active material is the positive electrode material described in the present invention.
[0092] According to an embodiment of the present invention, the positive electrode active material layer further includes a binder, and optionally further includes a positive electrode conductive material.
[0093] The binder improves the bonding of the positive electrode active material particles to each other and also improves the bonding of the positive electrode active material to the current collector. Non-limiting examples of binders include polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc.
[0094] The positive electrode active material layer includes a positive electrode conductive material to impart conductivity to the electrode. The positive electrode conductive material may include any conductive material as long as it does not cause chemical changes. Non-limiting examples of positive electrode conductive materials include carbon-based materials (e.g., natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, etc.), metal-based materials (e.g., metal powder, metal fiber, etc., including, for example, copper, nickel, aluminum, silver, etc.), conductive polymers (e.g., polyphenylene derivatives) and mixtures thereof.
[0095] The positive electrode collector for the secondary battery according to the present invention may be aluminum (Al), but is not limited thereto.
[0096] negative electrode
[0097] The negative electrode sheet generally includes a negative electrode current collector and a negative electrode active material layer located on the surface of the negative electrode current collector, and the negative electrode active material layer generally includes a negative electrode active material. The negative electrode active material can be various materials suitable for negative electrode active materials of lithium ion batteries in the art, for example, it can be one or more of graphite, soft carbon, hard carbon, carbon fiber, mesophase carbon microspheres, silicon-based materials, tin-based materials, lithium titanate or other metals that can form alloys with lithium. Among them, the graphite can be selected from one or more of artificial graphite, natural graphite and modified graphite; the silicon-based material can be selected from one or more of elemental silicon, silicon oxide compounds, silicon-carbon composites, and silicon alloys; the tin-based material can be selected from one or more of elemental tin, tin oxide compounds, and tin alloys. The negative electrode current collector is generally a structure or part that collects current. The negative electrode current collector can be various materials suitable for use as negative electrode current collectors of lithium ion batteries in the art. For example, the negative electrode current collector can be one or more of metal foil, and more specifically can be one or more of copper foil.
[0098] Preferably, the negative electrode adopts a silicon-carbon negative electrode. The present invention uses lithium-rich lithium ferrite to coat lithium manganese oxide to prepare a lithium-rich lithium manganese oxide positive electrode material, and uses it with a silicon-carbon negative electrode to obtain a long-cycle, high-energy-density battery. This is because the negative electrode adopts silicon-carbon material, which has a high gram capacity and low initial efficiency. A large amount of lithium needs to be consumed during the formation process. In order to improve the initial efficiency of the battery, lithium supplementation is required in the battery to reduce the consumption of lithium in the positive electrode, and lithium-rich lithium ferrite can be used as a lithium supplement additive.
[0099] Diaphragm
[0100] The isolation membrane can be any material suitable for lithium-ion battery separators in the art, for example, it can be a combination of one or more of polyethylene, polypropylene, polyvinylidene fluoride, aramid, polyethylene terephthalate, polytetrafluoroethylene, polyacrylonitrile, polyimide, polyamide, polyester and natural fiber, etc., but not limited to.
[0101] Electrolyte
[0102] The electrolyte that can be used in the embodiment of the present invention can be an electrolyte known in the prior art. The electrolyte that can be used in the electrolyte of the embodiment of the present invention includes, but is not limited to: inorganic lithium salts, such as LiClO4, LiPF6, LiBF4, LiSbF6, LiSO3F, LiN(FSO2)2, etc.; fluorine-containing organic lithium salts, such as LiCF3SO3, LiN(FSO2)(CF3SO2), LiN(CF3SO2)2, LiN(C2F5SO2)2, cyclic 1,3-hexafluoropropane disulfonyl imide lithium, cyclic 1,2-tetrafluoroethane disulfonyl imide lithium, LiC(CF3SO 2), LiPF4(CF3)2, LiPF4(C2F5)2, LiPF4(CF3SO2)2, LiPF4(C2F5SO2)2, LiBF2(CF3)2, LiBF2(C2F5)2, LiBF2(CF3SO2)2, LiBF2(C2F5SO2)2; lithium salts containing dicarboxylic acid complexes, such as lithium bis(oxalato)borate, lithium difluorooxalatoborate, lithium tris(oxalato)phosphate, lithium difluorobis(oxalato)phosphate, lithium tetrafluoro(oxalato)phosphate, etc. In addition, the above electrolytes can be used alone or in combination of two or more. For example, in some embodiments, the electrolyte includes a combination of LiPF6 and LiBF4. In some embodiments, the electrolyte includes a combination of an inorganic lithium salt such as LiPF6 or LiBF4 and a fluorine-containing organic lithium salt such as LiCF3SO3, LiN(CF3SO2)2, or LiN(C2F5SO2)2.
[0103] In some embodiments, the concentration of the electrolyte is in the range of 0.8mol / L to 3mol / L, for example, in the range of 0.8mol / L to 2.5mol / L, in the range of 0.8mol / L to 2mol / L, in the range of 1mol / L to 2mol / L, for example, 1mol / L, 1.15mol / L, 1.2mol / L, 1.5mol / L, 2mol / L or 2.5mol / L.
[0104] The solvents that can be used in the electrolyte of the embodiment of the present invention include, but are not limited to: carbonate compounds, ester-based compounds, ether-based compounds, ketone-based compounds, alcohol-based compounds, aprotic solvents, or combinations thereof.
[0105] Examples of the carbonate compound include, but are not limited to, a chain carbonate compound, a cyclic carbonate compound, a fluorinated carbonate compound, or a combination thereof.
[0106] Examples of chain carbonate compounds include, but are not limited to, diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC) and combinations thereof. Examples of cyclic carbonate compounds are ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinyl ethylene carbonate (VEC) and combinations thereof. Examples of fluorocarbonate compounds are fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, trifluoromethylethylene carbonate and combinations thereof.
[0107] The preparation of lithium-ion batteries is described below by taking lithium-ion batteries as an example and combining specific embodiments. Those skilled in the art will understand that the preparation method described in this application is only an example, and any other suitable preparation method is within the scope of this application.
[0108] Example 1
[0109] Lithium manganese oxide (LiMn2O4) and lithium-rich lithium iron oxide (Li5FeO4) are mixed in a mass ratio of 97:3, an appropriate amount of isopropanol is added, and the mixture is evenly mixed using a high-speed disperser. The mixture is vacuum dried at 200°C for 2 hours and ground to control the particle size to 50 nm to obtain a positive electrode material. The positive electrode is made of this material, and a battery is prepared in combination with a silicon-carbon negative electrode.
[0110] Example 2
[0111] Lithium manganese oxide (LiMn2O4) and lithium-rich lithium iron oxide (Li5FeO4) are mixed in a mass ratio of 90:10, an appropriate amount of isopropanol is added, and the mixture is evenly mixed using a high-speed disperser. The mixture is vacuum dried at 200°C for 2 hours and ground to control the particle size to 50nm to obtain a positive electrode material. The positive electrode is made of this material, and a battery is prepared in combination with a silicon-carbon negative electrode.
[0112] Example 3
[0113] Lithium manganese oxide (LiMn2O4) and lithium-rich lithium iron oxide (Li5FeO4) are mixed in a mass ratio of 95:5, an appropriate amount of isopropanol is added, and the mixture is evenly mixed using a high-speed disperser. The mixture is vacuum dried at 200°C for 2 hours and ground to control the particle size to 50 nm to obtain a positive electrode material. The positive electrode is made of this material, and a battery is prepared in combination with a silicon-carbon negative electrode.
[0114] Example 4
[0115] Lithium manganese oxide (LiMn2O4) and lithium iron oxide (Li5FeO4) were mixed in a mass ratio of 97:3, an appropriate amount of isopropanol was added, and the mixture was uniformly mixed using a high-speed disperser, dried at 200°C in vacuum for 2h, and ground to control the particle size to 50nm, thereby obtaining a positive electrode composite material;
[0116] The positive electrode composite material powder is added to the silk protein modified carbon nanotube solution. The mass ratio of the positive electrode composite material powder and the silk protein modified carbon nanotube solution is 1:2. The composite liquid is evenly stirred to obtain the composite liquid. The composite liquid is vacuum filtered and dried to obtain the positive electrode composite material uniformly coated with silk protein modified carbon nanotubes. The positive electrode is made of this material, and a battery is prepared in combination with a silicon-carbon negative electrode.
[0117] Example 5
[0118] Lithium manganese oxide (LiMn2O4) and lithium iron oxide (Li5FeO4) were mixed in a mass ratio of 97:3, an appropriate amount of isopropanol was added, and the mixture was uniformly mixed using a high-speed disperser, dried at 200°C in vacuum for 2h, and ground to control the particle size to 50nm, thereby obtaining a positive electrode composite material;
[0119] The positive electrode composite material powder is evenly mixed with a surfactant (SDS) solution and a template (SiO2 nanosphere) solution. The mass ratio of the positive electrode composite material, the surfactant solution and the template solution is 1.25:1:1. At 60°C and under stirring conditions, the composite material is self-assembled to form a composite material. The template is then removed with HF and dried to obtain a positive electrode composite material with a specific nanostructure. The positive electrode is made of this material, and a battery is prepared in combination with a silicon-carbon negative electrode.
[0120] Example 6
[0121] Lithium manganese oxide (LiMn2O4) and lithium iron oxide (Li5FeO4) were mixed in a mass ratio of 97:3, an appropriate amount of isopropanol was added, and the mixture was uniformly mixed using a high-speed disperser, dried at 200°C in vacuum for 2h, and ground to control the particle size to 50nm, thereby obtaining a positive electrode composite material;
[0122] The positive electrode composite material is immersed in a paraffin solution, the mass ratio of the positive electrode composite material to the paraffin solution is 1:5, and complete infiltration is ensured. After being taken out, it is dried at 50° C. for 2 hours to remove the surface ethanol, and a paraffin-coated composite material is obtained;
[0123] The coated composite material is dried at 50°C for 2 hours to ensure that the surface moisture or solvent is completely evaporated; then it is further dried at 90°C for 2 hours to obtain a modified positive electrode composite material, which is used to make a positive electrode and is combined with a silicon-carbon negative electrode to prepare a battery.
[0124] Comparative Example 1
[0125] Different from Example 1, pure lithium manganese oxide is used as the positive electrode and silicon carbon is used as the negative electrode, and the battery is manufactured according to the conventional method.
[0126] The batteries prepared in the above embodiments and comparative examples were tested for battery performance according to national standards. The test results are shown in Table 1 below.
[0127] Table 1
[0128] project Battery capacity Battery first effect Battery Energy Density Cycle capacity retention rate Example 1 1Ah 94% 210 80% / 1000cl Example 2 1Ah 95% 210 80% / 1500cl Example 3 1Ah 97% 210 80% / 1500cl Example 4 1Ah 98% 210 80% / 1500cl Example 5 1Ah 97% 220 80% / 1500cl Example 6 1Ah 94% 210 80% / 1300cl Comparative Example 1 1Ah 86% 190 80% / 500cl
[0129] As can be seen from Table 1 above, compared with the existing lithium-ion battery made of pure lithium manganese oxide positive electrode material, the lithium-ion battery of the present invention has effectively improved initial efficiency and battery energy density, and the cycle capacity is also improved. This shows that the present invention uses lithium-rich ferrite to coat lithium manganese oxide to form a positive electrode material, wherein the lithium-rich ferrite can be used as a lithium supplement additive, thereby effectively improving the cycle performance of lithium manganese oxide and improving the initial efficiency of the battery.
[0130] By comparing Example 1 and Example 4, it can be seen that the present invention can improve the conductivity and structural stability of the material by further introducing silk protein-modified carbon nanotubes for conductivity enhancement, which is beneficial to improving the first efficiency and cycle performance of the battery.
[0131] By comparing Example 1 and Example 5, it can be seen that the present invention further introduces self-assembly technology to prepare a positive electrode material with a specific nanostructure, which can increase the specific surface area and electrochemical performance of the material, thereby improving the first efficiency and energy density of the battery.
[0132] By comparing Example 1 and Example 6, it can be seen that the present invention can enhance the performance and safety of the battery under extreme conditions by further introducing phase change materials for coating, and helps to improve the cycle performance of the battery at high temperatures.
[0133] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs can also change and modify the above embodiment. Therefore, the present invention is not limited to the above specific embodiment, and any obvious improvement, replacement or modification made by those skilled in the art on the basis of the present invention belongs to the protection scope of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.
Claims
1. A method for preparing a positive electrode material for a battery that takes into account both initial efficiency and cycle performance, characterized in that: The positive electrode material includes LiMn2O4 and Li5FeO4 coated on the outer surface of the LiMn2O4; The method for preparing the positive electrode material comprises the following steps: Preparation of Li5FeO4: 1) mixing LiOH·H2O and Fe(NO3)3·9H2O at a molar ratio of Li:Fe of 8:1 to obtain a mixture; 2) Drying the mixed material; 3) Grind the mixed material and pre-sinter at a temperature of 400-600°C for 6-10 hours; 4) Grind and roast the mixed materials at a temperature of 800-1000°C for 8-20 hours; 5) grinding the product obtained in step 4) to obtain Li5FeO4; Preparation of positive electrode materials: a) mixing LiMn2O4 and Li5FeO4 in a mass ratio of 99:1 to 90:10; b) adding a dispersant, mixing evenly with a disperser, vacuum drying at 150-300° C. for 2-4 hours, and grinding to control the particle size to 10-90 nm, thereby obtaining a positive electrode composite material.
2. The method for preparing a positive electrode material for a battery having both initial efficiency and cycle performance according to claim 1, characterized in that: The method also includes the step of preparing LiMn2O4: mixing MnO2 and a lithium source according to a molar ratio of Mn:Li of 2:1.05, and sintering to obtain LiMn2O4.
3. The method for preparing a positive electrode material for a battery having both initial efficiency and cycle performance according to claim 1, characterized in that: The method also includes the step of preparing LiMn2O4: mixing Mn3O4 and a lithium source according to a molar ratio of Mn:Li of 2:1.05, and sintering to obtain LiMn2O4.
4. The method for preparing a positive electrode material for a battery having both initial efficiency and cycle performance as claimed in claim 1, characterized in that: In step 2) of preparing Li5FeO4, the drying temperature is 80-150°C and the time is 2-4h.
5. The method for preparing a positive electrode material for a battery having both initial efficiency and cycle performance as claimed in claim 1, characterized in that: In step b) of preparing the positive electrode material, the dispersant is at least one of isopropanol and ethanol.
6. The method for preparing a positive electrode material for a battery having both initial efficiency and cycle performance as claimed in claim 1, characterized in that: The preparation of the positive electrode material also includes step c): The positive electrode composite material powder is added to the silk protein modified carbon nanotube solution, the mass ratio of the positive electrode composite material powder to the silk protein modified carbon nanotube solution is 1: (1.8-2), the mixture is stirred evenly to obtain a composite solution, and the composite solution is vacuum filtered to obtain a composite material uniformly coated with the silk protein modified carbon nanotubes; Dry the filter cake at 80-90°C for 1-2 hours to remove surface moisture; The dried material is freeze-dried using a liquid nitrogen freeze dryer to ensure that the moisture inside the material is completely removed and its structural integrity is maintained; The dried material is further dried at 140-150° C. for 1-2 hours to obtain a modified positive electrode composite material.
7. The method for preparing a positive electrode material for a battery having both initial efficiency and cycle performance as claimed in claim 6, characterized in that: The preparation method of the silk protein modified carbon nanotube solution is: Adding multi-walled carbon nanotubes to deionized water, with a mass ratio of multi-walled carbon nanotubes to deionized water being 5:100, and ultrasonically treating for 30 to 40 minutes to obtain a uniformly dispersed carbon nanotube solution; Dissolve silk protein in deionized water, stir evenly, and prepare a silk protein solution with a mass concentration of 1%; The carbon nanotube solution is slowly added into the silk protein solution, and the mixture is continuously stirred and ultrasonically treated for 15 to 20 minutes to obtain a silk protein-modified carbon nanotube solution.
8. The method for preparing a positive electrode material for a battery having both initial efficiency and cycle performance as claimed in claim 1, characterized in that: The preparation of the positive electrode material also includes step d): The positive electrode composite material powder is uniformly mixed with the surfactant solution and the template solution, wherein the mass ratio of the positive electrode composite material, the surfactant solution and the template solution is 1.25:1:1, and the composite material having a nanostructure is self-assembled at 60° C. under stirring conditions; The self-assembled composite material was immersed in HF solution and stirred for 2 to 4 hours to ensure that the template was completely removed and the nanostructure was retained, and then filtered and washed with deionized water for multiple times to remove the residual HF; The filter cake is dried at 80°C for 2-3 hours to remove surface moisture; and then further dried at 150°C-300°C for 2-3 hours to obtain a positive electrode composite material with a nanostructure.
9. The method for preparing a positive electrode material for a battery having both initial efficiency and cycle performance as claimed in claim 8, characterized in that: The surfactant solution is a surfactant solution with a mass concentration of 2% formed by uniformly dispersing sodium dodecyl sulfate in deionized water; The template solution is a template solution with a mass concentration of 2% formed by uniformly dispersing SiO2 nanospheres in deionized water.
10. A battery positive electrode material that takes into account both initial efficiency and cycle performance, characterized in that: The positive electrode material is prepared by the method for preparing a positive electrode material for a battery that takes both initial efficiency and cycle performance into consideration as described in any one of claims 1 to 9.
Citation Information
Cited By
Method for repairing and regenerating waste lithium iron phosphate positive electrode material
CN121491123A