High-specific-surface layered oxide positive electrode material precursor for sodium-ion battery and preparation method and application of high-specific-surface layered oxide positive electrode material precursor
By using oxidizing gas to regulate the precursor morphology during the liquid phase co-precipitation of sodium ion batteries, the problem of insufficient high specific surface area of the positive electrode material of sodium ion batteries is solved, the electrochemical performance and high current capacity of the battery are improved, and it is suitable for industrialization Production.
Patent Information
- Application Number
- CN202411130937.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-08
AI Technical Summary
The existing precursors of layered oxide positive electrode materials of sodium ion batteries have a high specific surface area in the large-scale industrial production, resulting in low specific capacity and high current charging and discharging capabilities of the battery, making it difficult to improve electrochemical performance.
By introducing oxidative gas (air) during the liquid phase co-precipitation process and controlling the oxidative gas content in the reactor, the particle morphology refinement degree of sodium-electric precursor is regulated and its specific surface area is improved. It is suitable for the preparation of different series of Small-particle sodium-electric layered oxide positive electrode material precursor.
It significantly improves the specific surface area and electrochemical performance of the positive electrode material of sodium ion battery, enhances the specific capacity and high current charging and discharging capacity of the battery, is suitable for industrial mass production, and reduces costs.
Smart Images

Figure CN118908309A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a high surface area layered oxide positive electrode material precursor for sodium ion batteries, and a preparation method and application thereof. Background Art
[0002] In recent years, sodium-ion batteries have attracted increasing attention due to their cost and safety advantages. The key material of sodium-ion batteries is the cathode material, and the cost of the cathode material is one of the main factors determining the production cost of sodium-ion batteries. The development of advanced cathode materials with large-scale production capabilities is the key to realizing the commercial application of sodium-ion batteries.
[0003] Layered transition metal oxide cathode materials for sodium ion batteries (Na x TMO2 (TM = Fe, Mn, Ni, Cu, Zn, etc.) has the advantages of low cost, wide source of raw materials, simple synthesis process, easy large-scale industrial production, high energy density, high voltage platform, excellent comprehensive performance, and flexible chemical composition design. It is the mainstream research direction of positive electrode materials for sodium ion batteries. Among them, Fe, Mn, Ni, Cu, Zn, etc. are the best elements for constructing low-cost commercial layered oxide positive electrode materials.
[0004] Since the cathode material plays a decisive role in the performance of the battery, and the precursor directly determines the core electrochemical properties of the cathode material, the precursor of the layered oxide cathode material (Ni x TM 1-x The research on (OH)2)(0<x<1, TM=Fe, Mn, Cu, Zn, etc.) is of great significance to the development of sodium-ion batteries. At present, the precursors of layered oxide cathode materials for sodium-ion batteries are mainly produced in large quantities industrially by liquid phase co-precipitation method. Generally, the high specific surface area precursor materials have more voids and more ion transmission channels, which can effectively promote the deintercalation and extraction of ions, improve the specific capacity and high current charge and discharge capability of the material, and the rate performance of the battery. Therefore, the development of cathode material precursors with appropriate specific surface area is also crucial to improving the electrochemical performance of sodium-ion batteries.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] One of the purposes of the present invention is to provide a method for preparing a high specific surface area layered oxide positive electrode material precursor for a sodium ion battery. During the coprecipitation process, by introducing an oxidizing gas and controlling the oxidizing gas content in a reactor, the degree of refinement of the primary particle morphology of the sodium battery precursor can be effectively regulated. The obtained sodium battery precursor has a relatively refined particle morphology and a relatively high specific surface area, and is suitable for preparing different series of small-particle sodium battery layered oxide positive electrode material precursors.
[0007] The second object of the present invention is to provide a sodium ion battery positive electrode material, which is beneficial to improving the battery's specific capacity, large current charge and discharge capacity, and rate performance.
[0008] A third object of the present invention is to provide a sodium ion battery with excellent electrochemical performance.
[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0010] In a first aspect, a method for preparing a high surface area layered oxide positive electrode material precursor for a sodium ion battery comprises the following steps:
[0011] The mixed metal salt solution, the precipitant and the complexing agent are introduced into a reactor with a prepared base liquid to carry out a co-precipitation reaction, and the process parameters such as the reaction temperature, pH, the concentration of the complexing agent and the content of the oxidizing gas are controlled. Under the condition of an O2 volume content of 2.5±1.5%, the reaction is continued until the particle size of the product reaches the target particle size, thereby obtaining a sodium positive electrode material precursor;
[0012] In the granulation stage, the pH value in the reaction kettle is controlled to be a first pH value, the complexing agent value is a first complexing agent concentration value, and no oxidizing gas is introduced at this time; in the growth stage, the pH value in the reaction kettle is controlled to be a second pH value, the complexing agent value is a second complexing agent concentration value, and an oxidizing gas is gradually introduced at this time;
[0013] Wherein, 12.50>first pH value>second pH value>9.50, 0.01mol / L≤first complexing agent concentration value<second complexing agent concentration value≤1.0mol / L;
[0014] The oxidizing gas is air, and the volume content of O2 is controlled to be 2.5±1.5%.
[0015] Furthermore, the chemical composition of the positive electrode material precursor is as follows:
[0016] Ni x TM 1-x (OH)2(0<x<1, TM is a metal ion); wherein TM is selected from one or more of Fe, Mn, Cu and Zn.
[0017] Furthermore, the preparation method comprises the following steps:
[0018] (a) mixing metal salts according to the chemical composition of the cathode material precursor to obtain a mixed metal salt solution;
[0019] (b) The mixed metal salt solution of step (a) is first subjected to a nucleation reaction in the presence of a complexing agent and a precipitant, and then to a growth reaction, and a co-precipitation reaction is carried out under the condition of an O2 volume content of 2.5±1.5% until the D50 particle size of the product reaches the target particle size, and then the product is aged, centrifuged, dried, sieved, demagnetized and packaged in sequence to obtain a sodium positive electrode material precursor.
[0020] Furthermore, the D50 particle size of the sodium battery positive electrode material precursor is 3.0-6.0 um.
[0021] Further, the precipitant is sodium hydroxide solution;
[0022] Furthermore, the complexing agent is ammonia water or oxalic acid solution;
[0023] Further, the coprecipitation reaction temperature is 30-70°C;
[0024] Furthermore, the inert gas used in the reaction process is nitrogen.
[0025] In a second aspect, a sodium ion battery layered oxide positive electrode material precursor is prepared by any of the preparation methods described above.
[0026] Furthermore, the specific surface area of the positive electrode material precursor is 15-80m 2 / g.
[0027] In a third aspect, a sodium ion battery positive electrode material is prepared using the positive electrode material precursor described above, and the preparation method thereof comprises the following steps: the sodium positive electrode material precursor is uniformly mixed with a sodium source (NaOH, Na2CO3, etc.), and then calcined at a high temperature to obtain a sodium layered oxide positive electrode material Na(Ni x TM 1-x )O2(0<x<1).
[0028] In a fourth aspect, a sodium ion battery is provided, wherein the positive electrode of the sodium ion battery comprises the positive electrode material described above.
[0029] Compared with the prior art, the present invention has at least the following beneficial effects:
[0030] The present invention provides a method for preparing a high specific surface area layered oxide positive electrode material precursor for a sodium ion battery. By introducing an oxidizing gas (air) during a liquid phase coprecipitation process and controlling the oxidizing gas content in a reactor (the O2 volume content is 2.5±1.5%), the refinement degree of the primary particles of the sodium battery precursor is effectively regulated. The obtained small-particle sodium battery precursor has a relatively refined particle morphology and a relatively high specific surface area.
[0031] On the one hand, the introduction of an appropriate amount of oxidizing gas during the coprecipitation process can properly expand the layered structure of the precursor crystal particles, making the precursor primary particles loose, thereby refining the particle morphology, and finally obtaining a loose and porous precursor structure, significantly increasing the specific surface area of the precursor. At the same time, using air as the source of oxidizing gas can not only greatly save costs, but also easily achieve the refinement of the primary particle morphology of the sodium electrode precursor, which is suitable for industrial mass production.
[0032] On the other hand, the higher or lower the oxidizing gas content is, the better. When the oxygen content is too high, the oxidation degree of the precursor will deepen, and a large amount of Fe 2+ Oxidized to Fe 3+ , which leads to the formation of small balls, because Fe 2+ K sp About 4.87*10 -17 , while Fe 3+ K sp About 2.79*10 -39 , Fe 3+ It is very easy to be ahead of Ni 2+ , Mn 2+ When the oxygen content is too low, it cannot produce a significant refinement effect on the morphology of the precursor primary particles, and thus cannot effectively increase the specific surface area of the precursor.
[0033] At the same time, the preparation method of the present invention is suitable for preparing different series of small-particle sodium-electrolyte layered oxide positive electrode material precursors, such as nickel iron manganese (NiFeMn), nickel iron manganese copper (NiFeMnCu) and nickel iron manganese zinc (NiFeMnZn) series. It not only has a wide range of applications, but is also easy to operate and control, and is suitable for industrial production.
[0034] The sodium ion battery layered oxide positive electrode material precursor provided by the present invention has relatively refined particle morphology and relatively high specific surface area, and has good sphericity.
[0035] The sodium ion battery positive electrode material provided by the present invention is beneficial to improving the specific capacity, large current charge and discharge capacity and rate performance of the battery.
[0036] The sodium ion battery provided by the present invention has excellent electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0038] Figure 1 A flow chart for preparing a sodium electrode precursor provided in one embodiment of the present invention;
[0039] Figure 2 This is a SEM image of the sodium electrode precursor provided in Example 1 of the present invention;
[0040] Figure 3 This is a SEM image of the sodium electrode precursor provided in Example 2 of the present invention;
[0041] Figure 4 This is a SEM image of the sodium electrode precursor provided in Example 3 of the present invention;
[0042] Figure 5 This is a SEM image of the sodium electrode precursor provided in Example 4 of the present invention;
[0043] Figure 6 This is a SEM image of the sodium electrode precursor provided in Example 5 of the present invention;
[0044] Figure 7 This is a SEM image of the sodium electrode precursor provided in Comparative Example 1 of the present invention;
[0045] Figure 8 This is a SEM image of the sodium electrode precursor provided in Comparative Example 2 of the present invention;
[0046] Fig. 9 This is a SEM image of the sodium electrode precursor provided in Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0047] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0048] According to a first aspect of the present invention, there is provided a method for preparing a high surface area layered oxide positive electrode material precursor for a sodium ion battery, comprising the following steps:
[0049] The mixed metal salt solution, the precipitant and the complexing agent are introduced into a reactor with a prepared base liquid to carry out a co-precipitation reaction, and the process parameters such as the reaction temperature, pH, the concentration of the complexing agent and the content of the oxidizing gas are controlled. Under the condition of an O2 volume content of 2.5±1.5%, the reaction is continued until the particle size of the product reaches the target particle size, thereby obtaining a sodium positive electrode material precursor;
[0050] In the granulation stage, the pH value in the reaction kettle is controlled to be a first pH value, the complexing agent value is a first complexing agent concentration value, and no oxidizing gas is introduced at this time; in the growth stage, the pH value in the reaction kettle is controlled to be a second pH value, the complexing agent value is a second complexing agent concentration value, and an oxidizing gas is gradually introduced at this time;
[0051] Wherein, 12.50>first pH value>second pH value>9.50, 0.01mol / L≤first complexing agent concentration value<second complexing agent concentration value≤1.0mol / L;
[0052] The oxidizing gas is air, and the O2 volume content is controlled to be 2.5±1.5%.
[0053] The preparation method provided by the present invention introduces an oxidizing gas (air) during the liquid phase co-precipitation process. At a specific volume content of O2, the degree of refinement of the precursor primary particles can be effectively regulated, so that the prepared small-particle sodium electrode precursor has a relatively refined particle morphology and a relatively high specific surface area.
[0054] In the coprecipitation process, the typical but non-limiting volume content of O2 can be, for example, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, and 4%. The appropriate volume content of O2 in the reactor is more conducive to regulating the refinement of the precursor primary particles and ensuring that the sodium electrode precursor has a relatively refined particle morphology and a relatively high specific surface area. If the content of O2 in the reactor is too high, the oxidation degree of the precursor will be deepened, and a large amount of Fe 2+ Oxidized to Fe 3+ , which leads to small balls; if the O2 content in the reactor is too low, the primary particle morphology of the precursor cannot be significantly refined, and the specific surface area of the precursor cannot be effectively increased.
[0055] In the present invention, the source of O2 includes but is not limited to air; using air as the source of oxidizing gas can not only greatly save costs, but also easily achieve the refinement of the primary particle morphology of the sodium electrode precursor, with good sphericity, a wide range of applications, and is more suitable for industrial mass production.
[0056] At the same time, the preparation method of the present invention is suitable for preparing different series of small-particle sodium-electrolyte layered oxide positive electrode material precursors, such as nickel iron manganese (NiFeMn), nickel iron manganese copper (NiFeMnCu) and nickel iron manganese zinc (NiFeMnZn) series.
[0057] In a preferred embodiment, the chemical composition of the positive electrode material precursor is as follows:
[0058] Ni x TM 1-x (OH)2; wherein TM is selected from one or more of Fe, Mn, Cu and Zn.
[0059] In a preferred embodiment, the preparation method of the present invention comprises the following steps:
[0060] (a) mixing metal salts according to the chemical composition of the cathode material precursor to obtain a mixed metal salt solution;
[0061] (b) The mixed metal salt solution of step (a) is first subjected to a nucleation reaction in the presence of a complexing agent and a precipitant, and then to a growth reaction, and a co-precipitation reaction is carried out under the condition of an O2 volume content of 2.5±1.5% until the D50 particle size of the product reaches the target particle size, and then the product is aged, centrifuged, dried, sieved, demagnetized and packaged in sequence to obtain a sodium positive electrode material precursor.
[0062] The flow chart of the preparation method of the present invention is shown in Figure 1 , pump the mixed metal salt solution, complexing agent and precipitant into the reactor for mixing, control the process parameters such as reaction temperature, complexing agent concentration, pH value and stirring speed, and after the nucleation is completed, introduce oxidizing gas to continue the growth reaction, thereby effectively regulating the degree of refinement of the precursor primary particles, and carry out post-processing after reaching the target particle size, including aging, centrifugation, drying, screening, demagnetization and packaging in sequence, and finally obtain the sodium electric layered positive electrode material precursor after the physical and chemical indicators are tested to be qualified.
[0063] In a preferred embodiment, the temperature condition of the coprecipitation reaction can be 30-70°C, and typical but non-limiting temperatures can be, for example, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, and 70°C.
[0064] In summary, the preparation method provided by the present invention, under N2 protection, uses ammonia water or oxalic acid as a complexing agent, sodium hydroxide as a precipitant, and air as an oxidizing gas to carry out a liquid phase co-precipitation reaction. That is, under the condition that the process parameters are relatively fixed, the primary particles of the sodium electric precursor are mainly refined by regulating the content of the oxidizing gas in the reactor. The obtained sodium electric precursor has a relatively refined particle morphology and a relatively high specific surface area, good sphericity, and a wide range of applications.
[0065] According to a second aspect of the present invention, there is provided a sodium ion battery layered oxide positive electrode material precursor, which is prepared by any of the preparation methods described above and has a relatively refined particle morphology, a relatively high specific surface area, and good sphericity.
[0066] In the present invention, the D50 particle size of the cathode material precursor can be 3.0-6.0 μm, and the specific surface area can be 15-80 m 2 / g.
[0067] According to the third aspect of the present invention, there is provided a sodium ion battery layered positive electrode material, which is prepared using the high specific surface area positive electrode material precursor described above, has good electrochemical properties, and is beneficial to improving the battery's specific capacity, large current charge and discharge capability, and rate performance.
[0068] According to a fourth aspect of the present invention, a sodium ion battery is provided, wherein the positive electrode of the sodium ion battery comprises the positive electrode material described above and has excellent electrochemical performance.
[0069] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.
[0070] Example 1
[0071] A method for preparing a high surface area layered oxide positive electrode material precursor for a sodium ion battery comprises the following steps:
[0072] S1: pure water was added to the reactor and heated to 45°C, and nitrogen was introduced at a flow rate of 30 L / h, and then an ammonia solution was added to adjust the ammonium concentration of the bottom liquid to 0.30 mol / L, and then a sodium hydroxide solution was added to adjust the pH value of the bottom liquid to 11.30, and the stirring blade inside the reactor was stirred at a speed of 500 r / min to mix the bottom liquid uniformly to obtain the bottom liquid of the coprecipitation reaction;
[0073] S2: Pump 2.0 mol / L nickel-iron-manganese mixed salt solution, 11.0 mol / L sodium hydroxide solution and 7.5 mol / L ammonia solution into the above reactor at the same time, control the molar ratio of nickel-iron-manganese to be 33.3:33.3:33.3, and react for 1 hour under the conditions of maintaining the pH value at 11.30 and the ammonium concentration at 0.30 mol / L in the reactor to complete the nucleation task;
[0074] S3: After completing the nucleation task, the process is switched to a growth process, the pH value of the reactor is gradually reduced to 10.30, the ammonium concentration is increased to 0.40 mol / L, the reaction temperature is increased to 50°C, the speed is adjusted to 400 r / min, and air is introduced to control the O2 volume content in the reactor to 3.5±0.5%, and the reaction is continued until the D50 particle size of the product reaches 4.0 μm;
[0075] S4: The above products are pumped into an aging tank through a discharge port, and then aged, centrifuged, dried, screened, demagnetized and packaged to obtain a sodium-electro-nickel-iron-manganese ternary precursor (Ni 0.333 Fe 0.333 Mn 0.333 (OH)2), the scanning electron microscope image is as follows Figure 2 As shown in the figure, it can be seen that it has a relatively refined particle morphology, good sphericity, and a relatively high specific surface area (31.0m 2 / g).
[0076] Example 2
[0077] A method for preparing a high surface area layered oxide positive electrode material precursor for a sodium ion battery comprises the following steps:
[0078] S1: pure water was added to the reactor and heated to 40°C, and nitrogen was introduced at a flow rate of 30 L / h, and then oxalic acid solution was added to adjust the oxalate concentration of the bottom liquid to 0.10 mol / L, and then sodium hydroxide solution was added to adjust the pH value of the bottom liquid to 11.60, and the stirring blade inside the reactor was stirred at a speed of 500 r / min to mix the bottom liquid evenly to obtain the bottom liquid of the coprecipitation reaction;
[0079] S2: Pump 2.0 mol / L nickel-iron-manganese-copper mixed salt solution, 11.0 mol / L sodium hydroxide solution and 1.5 mol / L oxalic acid solution into the above reactor at the same time, control the molar ratio of nickel-iron-manganese-copper to be 22:22:43.8:12.2, and react for 1 hour under the conditions of maintaining the pH value at 11.60 and the oxalate concentration at 0.10 mol / L in the reactor to complete the nucleation task;
[0080] S3: After completing the nucleation task, the process is switched to a growth process, the pH value of the reactor is gradually reduced to 11.30, the oxalate concentration is increased to 0.40 mol / L, the reaction temperature is increased to 60°C, the speed is adjusted to 400 r / min, and air is introduced to control the O2 volume content in the reactor to 3.5±0.5%, and the reaction is continued until the D50 particle size of the product reaches 4.0 μm;
[0081] S4: The above products are pumped into an aging tank through a discharge port, and then aged, centrifuged, dried, screened, demagnetized and packaged to obtain a sodium-electro-nickel-iron-manganese-copper quaternary precursor (Ni0.22 Fe 0.22 Mn 0.438 Cu 0.122 (OH)2), the scanning electron microscope image is as follows Figure 3 As shown in the figure, it can be seen that it has a relatively refined particle morphology, good sphericity, and a relatively high specific surface area (76.94m 2 / g).
[0082] Example 3
[0083] A method for preparing a high surface area layered oxide positive electrode material precursor for a sodium ion battery comprises the following steps:
[0084] S1: pure water was added to the reactor and heated to 40°C, and nitrogen was introduced at a flow rate of 30 L / h, and then oxalic acid solution was added to adjust the oxalate concentration of the bottom liquid to 0.10 mol / L, and then sodium hydroxide solution was added to adjust the pH value of the bottom liquid to 11.60, and the stirring blade inside the reactor was stirred at a speed of 500 r / min to mix the bottom liquid evenly to obtain the bottom liquid of the coprecipitation reaction;
[0085] S2: Pump 2.0 mol / L nickel-iron-manganese-zinc mixed salt solution, 11.0 mol / L sodium hydroxide solution and 1.5 mol / L oxalic acid solution into the above reactor at the same time, control the molar ratio of nickel-iron-manganese-zinc to be 23.2:31.8:37.3:7.8, and react for 1 hour under the conditions of maintaining the pH value at 11.60 and the oxalate concentration at 0.10 mol / L in the reactor to complete the nucleation task;
[0086] S3: After completing the nucleation task, the process is switched to a growth process, the pH value of the reactor is gradually reduced to 11.30, the oxalate concentration is increased to 0.40 mol / L, the reaction temperature is increased to 60°C, the speed is adjusted to 400 r / min, and air is introduced to control the O2 volume content in the reactor to 3.5±0.5%, and the reaction is continued until the D50 particle size of the product reaches 4.0 μm;
[0087] S4: The above products are pumped into an aging tank through a discharge port, and then aged, centrifuged, dried, screened, demagnetized and packaged to obtain a sodium-electro-nickel-iron-manganese-zinc quaternary precursor (Ni 0.232 Fe 0.318 Mn 0.373 Zn 0.078 (OH)2), the scanning electron microscope image is as follows Figure 4 As shown in the figure, it can be seen that it has a relatively refined particle morphology, good sphericity, and a relatively high specific surface area (57.22m 2 / g).
[0088] Example 4
[0089] The difference between this embodiment and embodiment 1 is that in step S3, the volume content of O2 in the reactor is controlled to be 1.5±0.5%;
[0090] The remaining steps and process parameters are the same as those in Example 1 to obtain a sodium-electro-nickel-iron-manganese ternary precursor (Ni 0.333 Fe 0.333 Mn 0.333 (OH)2), the scanning electron microscope image is as follows Figure 5 As shown in the figure, compared with the original sample, its particle morphology is obviously finer and its specific surface area is relatively higher (15.26m 2 / g).
[0091] Example 5
[0092] The difference between this embodiment and embodiment 1 is that in step S3, the volume content of O2 in the reactor is controlled to be 2.5±0.5%;
[0093] The remaining steps and process parameters are the same as those in Example 1 to obtain a sodium-electro-nickel-iron-manganese ternary precursor (Ni 0.333 Fe 0.333 Mn 0.333 (OH)2), the scanning electron microscope image is as follows Figure 6 As shown in the figure, compared with the original sample, its particle morphology is more refined and its specific surface area is higher (21.50m 2 / g).
[0094] Comparative Example 1
[0095] A method for preparing a layered oxide positive electrode material precursor for a sodium ion battery comprises the following steps:
[0096] S1: pure water was added to the reactor and heated to 45°C, and nitrogen was introduced at a flow rate of 30 L / h, and then an ammonia solution was added to adjust the ammonium concentration of the bottom liquid to 0.30 mol / L, and then a sodium hydroxide solution was added to adjust the pH value of the bottom liquid to 11.30, and the stirring blade inside the reactor was stirred at a speed of 500 r / min to mix the bottom liquid uniformly to obtain the bottom liquid of the coprecipitation reaction;
[0097] S2: Pump 2.0 mol / L nickel-iron-manganese mixed salt solution, 11.0 mol / L sodium hydroxide solution and 7.5 mol / L ammonia solution into the above reactor at the same time, control the molar ratio of nickel-iron-manganese to be 33.3:33.3:33.3, and react for 1 hour under the conditions of maintaining the pH value at 11.30 and the ammonium concentration at 0.30 mol / L in the reactor to complete the nucleation task;
[0098] S3: After completing the nucleation task, the process is switched to a growth process, the pH value of the reactor is gradually reduced to 10.30, the ammonium concentration is increased to 0.40 mol / L, the reaction temperature is increased to 50°C, the speed is adjusted to 400 r / min, and the reaction is continued until the D50 particle size of the product reaches 4.0 μm;
[0099] S4: The above products are pumped into an aging tank through a discharge port, and then aged, centrifuged, dried, screened, demagnetized and packaged to obtain a sodium-electro-nickel-iron-manganese ternary precursor (Ni 0.333 Fe 0.333 Mn 0.333 (OH)2), the scanning electron microscope image is as follows Figure 7 As shown in the figure, the particle morphology is obviously thick strip, and the specific surface area is relatively low (9.87m 2 / g).
[0100] Comparative Example 2
[0101] The difference between this comparative example and Example 1 is that in step S3, the volume content of O2 in the reactor is controlled to be 0.75±0.25%;
[0102] The remaining steps and process parameters are the same as those in Example 1 to obtain a sodium-electro-nickel-iron-manganese ternary precursor (Ni 0.333 Fe 0.333 Mn 0.333 (OH)2), the scanning electron microscope image is as follows Figure 8 As shown in the figure, compared with the original sample, its particle morphology is slightly finer and its specific surface area is slightly higher (11.60m 2 / g).
[0103] Compared with Example 1, the volume content of O2 in the reactor in this comparative example is too low, which will result in the inability to effectively refine the primary particle morphology of the precursor, thereby failing to effectively increase the specific surface area of the precursor.
[0104] Comparative Example 3
[0105] The difference between this comparative example and Example 1 is that in step S3, the volume content of O2 in the reactor is controlled to be 5.0±1%;
[0106] The remaining steps and process parameters are the same as those in Example 1 to obtain a sodium-electro-nickel-iron-manganese ternary precursor (Ni 0.333 Fe 0.333 Mn 0.333 (OH)2), the scanning electron microscope image is as follows Fig. 9 As shown, compared with the original sample, a large number of small balls can be seen.
[0107] Compared with Example 1, the volume content of O2 in the reactor in this comparative example is too high, which will lead to excessive oxidation of the precursor and a large amount of Fe2+ Oxidized to Fe 3+ , resulting in a large number of small balls appearing in the reaction system, and the product cannot grow further.
[0108] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a high surface area layered oxide positive electrode material precursor for a sodium ion battery, characterized in that: The steps include: The mixed metal salt solution, the precipitant and the complexing agent are introduced into a reactor with a prepared base liquid to carry out a co-precipitation reaction, and the process parameters such as the reaction temperature, pH, the concentration of the complexing agent and the content of the oxidizing gas are controlled. Under the condition of an O2 volume content of 2.5±1.5%, the reaction is continued until the particle size of the product reaches the target particle size, thereby obtaining a sodium positive electrode material precursor; In the granulation stage, the pH value in the reaction kettle is controlled to be a first pH value, the complexing agent value is a first complexing agent concentration value, and no oxidizing gas is introduced at this time; in the growth stage, the pH value in the reaction kettle is controlled to be a second pH value, the complexing agent value is a second complexing agent concentration value, and an oxidizing gas is gradually introduced at this time; Wherein, 12.50>first pH value>second pH value>9.50, 0.01mol / L≤first complexing agent concentration value<second complexing agent concentration value≤1.0mol / L; The oxidizing gas is air, and the volume content of O2 is controlled to be 2.5±1.5%.
2. The preparation method according to claim 1, characterized in that: The chemical composition of the sodium cathode material precursor is as follows: Ni x TM 1-x (OH)2(0<x<1, TM is a metal ion); wherein TM is selected from one or more of Fe, Mn, Cu and Zn.
3. The preparation method according to claim 2, characterized in that: The preparation method comprises the following steps: (a) mixing metal salts according to the chemical composition of the cathode material precursor to obtain a mixed metal salt solution; (b) The mixed metal salt solution of step (a) is first subjected to a nucleation reaction in the presence of a complexing agent and a precipitant, and then to a growth reaction, and a co-precipitation reaction is carried out under the condition of an O2 volume content of 2.5±1.5% until the D50 particle size of the product reaches the target particle size, and then the product is aged, centrifuged, dried, sieved, demagnetized and packaged in sequence to obtain a sodium positive electrode material precursor.
4. The preparation method according to claim 3, characterized in that: The D50 particle size of the sodium positive electrode material precursor is 3.0-6.0 um.
5. The preparation method according to claim 3, characterized in that: The precipitant is sodium hydroxide or potassium hydroxide solution; Preferably, the complexing agent is ammonia water or oxalic acid solution; Preferably, the reaction temperature is 30-70°C; Preferably, the inert gas used in the reaction process is nitrogen or argon.
6. The preparation method according to claim 5, characterized in that: The precipitant is sodium hydroxide solution, the complexing agent is ammonia water or oxalic acid solution, and the inert gas is nitrogen.
7. A sodium ion battery layered oxide positive electrode material precursor, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 6.
8. The cathode material precursor according to claim 7, characterized in that: The specific surface area of the positive electrode material precursor is 15-80m 2 / g.
9. A sodium ion battery positive electrode material, characterized in that: The positive electrode material precursor according to claim 8 is prepared, and the preparation method thereof comprises the following steps: the positive electrode material precursor is uniformly mixed with a sodium source, and then calcined at a high temperature to obtain a sodium-electrolyte layered oxide positive electrode material Na(Ni x TM 1-x )O2(0<x<1).
10. A sodium ion battery, characterized in that: The positive electrode of the sodium ion battery comprises the positive electrode material according to claim 9.