High-gloss opaque glaze for sanitary ware ceramic as well as preparation method and application of high-gloss opaque glaze
By using barium frit and oxide combination in ceramic glaze, the shortage of zinc oxide resources and alternative materials are solved, the gloss and stability of the glaze is improved, and the melting effect is achieved that is consistent with zinc oxide is achieved. The problem of unstable glossiness of ceramic glaze.
Patent Information
- Application Number
- CN202411261753.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The commonly used zinc oxide resources in existing ceramic glazes are scarce, and their alternative materials such as strontium carbonate, barium carbonate and barium oxide have problems such as scarcity of resources, toxicity and energy waste, resulting in unstable gloss effect on the ceramic glaze.
Barium frit is used as the raw material of glaze, including the BaO-Na2O-SiO2 ternary system, and through specific glaze slurry preparation methods and firing conditions, combining barium oxide and other oxides, reducing the fusion temperature of barium oxide and improving glaze Surface gloss.
The glossiness of the gloss is improved and the stability of the glossiness of the gloss is avoided, and the defects of other alternative materials are achieved, and the melting effect is consistent with zinc oxide, which is rich in resources and environmentally friendly.
Smart Images

Figure BDA0005035900580000031 
Figure BDA0005035900580000041
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sanitary ceramics, and in particular relates to a high-gloss opalescent glaze for sanitary ware ceramics and a preparation method and application thereof. Background Art
[0002] In the manufacturing process of ceramic products, in order to obtain a high-gloss glaze, heavy metal oxides are added to the formula to help the glaze melt and enhance its gloss. Lead-containing glazes will inevitably dissolve lead during use, and long-term use will lead to lead poisoning, which is harmful to the health of users and has been banned; zinc oxide, as a metal element oxide with a high refractive index and excellent high-temperature fluxing effect, has become the main material for glaze gloss adjustment and fluxing in the industry and has been widely used.
[0003] Due to the continuous development of the use of zinc oxide materials, the application field of zinc oxide is becoming more and more extensive, resulting in the current shortage of zinc oxide resources. As a possible alternative material for zinc oxide, strontium carbonate cannot be widely used because of its low firing temperature and is greatly affected by the temperature fluctuation of the kiln; barium carbonate is toxic and harmful to the human body, so it is not suitable for large-scale production and use; the sulfide generated by the high-temperature decomposition of barium sulfate will cause serious corrosion damage to the kiln exhaust system if used in large quantities for a long time; barium oxide will increase the glaze slurry maturation temperature (zinc oxide can play a fluxing role at around 700°C, while barium oxide will only start to play a fluxing role at around 900°C), waste energy, and increase the amount of use will cause the glaze slurry to crystallize and lose its luster; resulting in barium oxide cannot be effectively used in ceramic glazes. Summary of the invention
[0004] The purpose of the present invention is to overcome the deficiencies of the prior art, provide a high-gloss opalescent glaze for sanitary ware ceramics and a preparation method and application thereof, and solve the problems in the above-mentioned background technology.
[0005] One of the technical solutions adopted by the present invention to solve the technical problem is: a high-gloss opalescent glaze for sanitary ware ceramics is provided, wherein the glaze slurry raw materials are composed by weight: 25-32 parts of quartz, 10-23 parts of potassium feldspar, 8-15 parts of calcite, 0-4 parts of dolomite, 1-6 parts of aluminum oxide, 2-5 parts of kaolin, 8-10 parts of zirconium silicate, 6-8 parts of wollastonite, 5-18 parts of albite, and 5-23 parts of barium frit.
[0006] In a preferred embodiment of the present invention, the barium frit contains a BaO-Na2O-SiO2 ternary system.
[0007] In a preferred embodiment of the present invention, the raw materials of the barium frit are composed of silicon dioxide, aluminum oxide, calcium oxide, magnesium oxide, potassium oxide, sodium oxide, zinc oxide and barium oxide.
[0008] In a preferred embodiment of the present invention, the raw materials of the barium frit include, by mass, 44-45 parts of silicon dioxide, 20-21 parts of aluminum oxide, 14-15 parts of calcium oxide, 3-5 parts of magnesium oxide, 4-5 parts of potassium oxide, 1-2 parts of sodium oxide, 0-0.1 parts of zinc oxide, and 9-10 parts of barium oxide.
[0009] The second technical solution adopted by the present invention to solve the technical problem is: a method for preparing high-gloss opalescent glaze for sanitary ware ceramics is provided, comprising the following steps:
[0010] 1) Mix the above glaze slurry raw materials with water and grind them into a mill to a cumulative particle size of 70-72% of 10 microns;
[0011] 2) The glaze slurry is refined and iron removed through a screen, and CMC is added for initial performance adjustment;
[0012] 3) After the initial adjustment of the glaze slurry properties, it is refined and iron-removed through a screen again, and a debonding agent is added to fine-tune the glaze slurry properties. The specific properties are: concentration 348-352 g / 200 mL, drying time to 17-23 minutes, viscosity 100-120 seconds / 200 mL, and yield value 15-25.
[0013] In a preferred embodiment of the present invention, in step 1), the glaze slurry raw materials are mixed in a mass ratio of glaze: ball: water = 1:1.8:0.46, and 0.12% of soda ash by mass of the glaze is added, and ball milling is performed for 8-9 hours using a drum ball mill.
[0014] In a preferred embodiment of the present invention, in step 2), the glaze is refined twice through a 200-mesh screen and an iron remover, and 0.25 parts by weight of CMC is added per 100 parts by weight of dry weight of the glaze for initial adjustment.
[0015] In a preferred embodiment of the present invention, in step 3), after the glaze slurry properties are initially adjusted, the glaze slurry is refined once again through a 200-mesh sieve, and a degumming agent is added to finely adjust the glaze slurry properties.
[0016] In a preferred embodiment of the present invention, the qualified glaze slurry is placed in a low-temperature chamber for storage and standby use.
[0017] The third technical solution adopted by the present invention to solve its technical problem is: to provide an application of high-gloss opalescent glaze for sanitary ware ceramics, using the above-mentioned glaze slurry to glaze the green bricks, the glazing thickness is 0.8-0.9mm, the firing temperature is 1225-1235℃, and the firing cycle is 14 hours.
[0018] Compared with the background technology, this technical solution has the following advantages:
[0019] 1. The present invention overcomes the negative problems of directly using materials such as barium carbonate or barium sulfate by introducing barium oxide in the form of a frit; in addition, the present invention utilizes the BaO-Na2O-SiO2 ternary system in the barium frit to generate a Ba-containing melt at 600-700°C, which, combined with the added albite, effectively reduces the fluxing temperature of simply using barium oxide, and promotes its fluxing effect to be consistent with that of zinc oxide, further overcoming the problems of relatively insufficient fluxing effect of barium itself, insufficient glaze vitrification, and insufficient glaze gloss enhancement.
[0020] 2. The barium oxide in the raw material of the present invention has relatively few current application fields, is rich in resources, has a high refractive index, a wide high-temperature adaptability range, is less affected by kiln fluctuations, and has a more stable glaze gloss. DETAILED DESCRIPTION
[0021] The present invention is further explained below in conjunction with specific examples and comparative examples. The raw material components in the following examples or comparative examples are shown in Table 1.
[0022] Table 1. Raw material composition
[0023]
[0024]
[0025] The raw material formula ratios of the glaze slurries of Examples 1-3 of the present invention and Comparative Examples 1-2 are shown in Table 2 (by mass).
[0026] Table 2
[0027] raw material Comparative Example 1 Comparative Example 2 Example 1 Example 2 Example 3 quartz 29 27 27 30 31 Potassium feldspar 31 - 20 13 12 Calcite 15.5 14.5 8 11 13 dolomite 4.5 - - 3 2 Burnt Talc - 2 - - - Alumina 3 - 2 4 5 Kaolin 3 8 4 4 2 Zirconium silicate 10.5 11 8 8 8 Wollastonite - - 6 6 7 Sodium feldspar - 34 5 10 15 Zinc Oxide 3.5 2 - - - Strontium carbonate - 1.5 - - - Ba frit - - 20 11 5 total 100 100 100 100 100
[0028] The glaze is prepared according to the formula ratio in Table 2. The preparation method includes the following steps:
[0029] 1) Weigh various raw materials according to the proportions in Table 2 and mix them; add 46 parts of water and 0.12 parts of soda ash per 100 parts of dry weight of glaze and grind them into a 10 micron cumulative particle size of 71-72%;
[0030] 2) After the glaze slurry is milled, it is refined twice through a 200-mesh screen and an iron remover, and 0.25 parts of CMC are added for each 100 parts of dry weight of the glaze for initial adjustment;
[0031] 3) After the initial adjustment, the glaze is refined again through a 200-mesh screen and an iron remover, and a debonding agent is added to finely adjust the glaze slurry. The modulation performance is: concentration 350g / 200ml, drying time to 17-23 minutes, viscosity 100-120 seconds / 200ml, and yield value 15-25 for standby use;
[0032] 4) Prepare 100mm*100mm green bricks and glaze them with the prepared glaze slurry with a glaze thickness of 0.8-0.9mm;
[0033] 5) Place the high-quality glazed tiles into a kiln for firing (firing temperature 1225-1235°C, firing cycle 14 hours). The glazed tile surface test results are shown in Table 3.
[0034] Table 3
[0035] performance Market products Comparative Example 1 Comparative Example 2 Example 1 Example 2 Example 3 Glazed pores 1-10 6 2 5 3 6 Glossiness 55-60 59.3 60 59.7 59.3 58.9 Roughness 0.060-0.110 0.065 0.110 0.058 0.060 0.056 Whiteness 69-79 78.2 79 76.4 75.7 75.3
[0036] It can be seen from Table 3 that the glaze effects of the glazed tiles of Examples 1-3 have reached the high-end level of high-gloss opalescent glazes in the current market.
[0037] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A high gloss opalescent glaze for sanitary ware ceramics. It is characterized in that The glaze slurry raw materials are composed of 25-32 parts of quartz, 10-23 parts of potassium feldspar, 8-15 parts of calcite, 0-4 parts of dolomite, 1-6 parts of aluminum oxide, 2-5 parts of kaolin, 8-10 parts of zirconium silicate, 6-8 parts of wollastonite, 5-18 parts of albite and 5-23 parts of barium frit.
2. A high gloss opalescent glaze for sanitary ware ceramics according to claim 1, Features: The barium frit contains BaO-Na 2 O-SiO 2 Ternary system.
3. A high gloss opalescent glaze for sanitary ware ceramics according to claim 1, Features: The raw materials of the barium frit are composed of silicon dioxide, aluminum oxide, calcium oxide, magnesium oxide, potassium oxide, sodium oxide, zinc oxide and barium oxide.
4. The high gloss opalescent glaze for sanitary ware ceramics according to claim 1, Features: The raw materials of the barium frit include, by mass, 44-45 parts of silicon dioxide, 20-21 parts of aluminum oxide, 14-15 parts of calcium oxide, 3-5 parts of magnesium oxide, 4-5 parts of potassium oxide, 1-2 parts of sodium oxide, 0-0.1 parts of zinc oxide, and 9-10 parts of barium oxide.
5. A method for preparing high-gloss opalescent glaze for sanitary ware ceramics, It is characterized in that The steps include: 1) Mixing the glaze slurry raw material according to claim 1 with water and grinding it to a cumulative particle size of 70-72% of 10 microns; 2) The glaze slurry is refined and iron removed through a screen after being milled, and CMC is added for initial performance adjustment; 3) After the initial adjustment of the glaze slurry properties, it is refined and iron-removed through a screen again, and a debonding agent is added to fine-tune the glaze slurry properties. The specific properties are: concentration 348-352 g / 200 mL, drying time to 17-23 minutes, viscosity 100-120 seconds / 200 mL, and yield value 15-25.
6. The method for preparing a high-gloss opalescent glaze for sanitary ware ceramics according to claim 5, Features: In step 1), the glaze slurry raw materials are mixed in a mass ratio of glaze: ball: water = 1:1.8:0.46, and 0.12% of soda ash by mass of the glaze is added, and the mixture is ball milled for 8-9 hours using a drum ball mill.
7. The method for preparing a high-gloss opalescent glaze for sanitary ware ceramics according to claim 5, Features: In step 2), the glaze is refined twice through a 200-mesh screen and an iron remover, and 0.25 parts by weight of CMC is added per 100 parts by weight of dry weight of the glaze for initial adjustment.
8. The method for preparing a high-gloss opalescent glaze for sanitary ware ceramics according to claim 5, Features: In step 3), after the glaze slurry properties are initially adjusted, the glaze slurry is refined once again through a 200-mesh sieve, and a degumming agent is added to finely adjust the glaze slurry properties.
9. The method for preparing a high-gloss opalescent glaze for sanitary ware ceramics according to claim 5, Features: The qualified glaze slurry is placed in a low-temperature chamber for storage and later use.
10. Application of a high-gloss opalescent glaze for sanitary ware ceramics, Features: The green brick pieces are glazed with the glaze slurry prepared with the raw materials according to claim 1, the glaze thickness is 0.8-0.9mm, the firing temperature is 1225-1235℃, and the firing cycle is 14 hours.
Citation Information
Patent Citations
Self-cleaning glaze repairing glaze for sanitary ceramics and preparation and use thereof
CN110171927A
White opaque glaze, white opaque glaze ceramic product and preparation method thereof
CN110482863A
Matte glaze and preparation method thereof
CN110510876A
Low-zirconium white glaze for sanitary ceramic and preparation process of low-zirconium white glaze
CN110627361A
FFC glaze with high stain resistance, FFC sanitary ceramic and preparation method of FFC sanitary ceramic
CN111253071A