Lime kiln capable of slowing down ring formation and calcination method

By setting up lifting bricks and castables in the lime kiln, the high-temperature knot ring problem caused by the concentration of the calcining section is solved, the thermal environment and production stability of the lime kiln are improved, the service life of the refractory material is extended, and the production and Maintenance cost.

CN118908599APending Publication Date: 2024-11-08XINXING DUCTILE IRON PIPES XINJIANG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410994147.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The temperature of the lime kiln calcining section is too concentrated, which leads to high-temperature knots, which increases the movement resistance of gases and materials, deteriorates the thermal environment, and reduces output and quality.

Method used

The lime kiln is equipped with pickup bricks in the preheating and calcining areas, and the castable material is filled in the adjacent areas. The lime stone blocks are turned over and fully contacted with high-temperature gas through the pickup bricks, and distributed evenly to avoid excessive local temperatures, and combined with reasonable The kiln body spacing and temperature settings extend the service life of the refractory material.

Benefits of technology

Significantly reduce the movement resistance of gases and materials, improve the thermal environment in lime kilns, improve the production stability and output of lime kilns, extend the service life of refractory materials, and reduce production and maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908599A_ABST
    Figure CN118908599A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of lime kilns, and particularly discloses a lime kiln capable of slowing down ring formation, which comprises a kiln body, a plurality of raising bricks are arranged in the kiln body, a hot work area in the kiln body is composed of a preheating area, a calcining area and a discharging area, the raising bricks are positioned in the preheating area and the calcining area of the kiln body, and a castable is filled between two adjacent raising bricks. The problems that in the using process of the lime kiln, the temperature of a calcination section is too concentrated, high-temperature ring forming occurs in the calcination section of the lime kiln, and therefore movement resistance of gas and materials is increased, the thermal environment in the lime kiln is deteriorated, and the yield and quality are reduced are solved. By arranging the raising bricks, the problem of high-temperature ring formation caused by temperature concentration of a calcining section during use of the lime kiln is successfully solved, the motion resistance of gas and materials is remarkably reduced, the thermal environment in the lime kiln is improved, and a guarantee is provided for stable production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lime kilns, and in particular to a lime kiln capable of slowing down ring formation and a calcining method. Background Art

[0002] A lime kiln is a device used to burn lime. Its main function is to calcine limestone (mainly calcium carbonate) under high temperature conditions to cause a chemical reaction and decompose it into quicklime (mainly calcium oxide) and carbon dioxide. There are various types of lime kilns, including vertical kilns and rotary kilns. Different types of lime kilns differ in structure, working principle and performance characteristics, but their basic purpose is to achieve effective calcination of limestone by controlling temperature, ventilation and other conditions to produce lime products that meet the requirements.

[0003] The overall structure of the current lime kiln is divided into a discharging section, a preheating section and a calcining section according to the temperature. Its working principle is mainly based on the thermal decomposition reaction of limestone. First, limestone raw materials that meet certain particle size requirements are added into the kiln from the top of the kiln, and then high temperature is generated through the combustion device at the bottom of the kiln (such as burning coal, gas, etc.). Hot air rises in the kiln. When the limestone is heated in the kiln to a certain temperature, a decomposition reaction occurs: CaCO3 (limestone) → CaO (quicklime) + CO2↑.

[0004] During the decomposition process of limestone, the temperature in the calcining section is too concentrated, resulting in high-temperature ringing in the calcining section of the lime kiln. Ringing mostly occurs in the high-temperature zone, which will reduce the cross-sectional area of ​​the lime kiln, thereby increasing the movement resistance of gas and materials, causing the temperature of the high-temperature zone to further rise, resulting in the deterioration of the thermal environment in the lime kiln and reducing production and quality. Summary of the invention

[0005] The object of the present invention is to provide a lime kiln and a calcining method for slowing down ring formation, so as to solve the problem that during the use of the lime kiln, the temperature in the calcining section is too concentrated, which will cause high-temperature ring formation in the calcining section of the lime kiln, thereby increasing the movement resistance of gas and materials, causing the thermal environment in the lime kiln to deteriorate, and reducing the output and quality.

[0006] In order to achieve the above-mentioned purpose, the basic solution provided by the present invention is: a lime kiln for slowing down ring formation, comprising a kiln body, wherein a plurality of lifting bricks are arranged in the kiln body, the thermal zone in the kiln body is composed of a preheating zone, a calcining zone and a discharge zone, the lifting bricks are located in the preheating zone and the calcining zone of the kiln body, and castables are filled between two adjacent lifting bricks.

[0007] The working principle of the present invention is that when the lime kiln needs to be used, first the limestone blocks enter the preheating zone of the kiln body for preheating. Under the rotation of the kiln body, the limestone blocks in the preheating zone of the kiln body are lifted up by the lifting bricks and turned over to fully contact with the high-temperature gas. At the same time, the limestone blocks roll from the preheating zone of the kiln body to the calcining zone of the kiln body. The limestone blocks entering the calcining zone of the kiln body are lifted up by the lifting bricks and turned over. The high-temperature flame calcines and decomposes the limestone. At the same time, the limestone blocks roll from the calcining zone of the kiln body to the discharging zone of the kiln body. After the limestone blocks enter the discharging zone, active lime products are obtained, which are transported to the crushing system through a chain conveyor and ground into active lime powder.

[0008] The beneficial effects of the present invention are as follows: by arranging the lifting bricks, the problem of high-temperature ringing caused by the concentrated temperature in the calcining section of the lime kiln during use is successfully solved, the movement resistance of gas and materials is significantly reduced, the thermal environment in the lime kiln is improved, and a guarantee is provided for stable production; secondly, by arranging the castable, the service life of the refractory materials in the rotary kiln is increased, the relative displacement friction and wear between the limestone and the internal refractory materials is reduced, and the production cost and maintenance cost are reduced.

[0009] Option 2 is a preferred option of the basic option. Upper and lower positioning grooves are provided on both sides of the lifting brick respectively. The upper and lower positioning grooves are provided on the lifting brick to enhance the stability of the castable and enable the castable to be more firmly attached to the lifting brick.

[0010] Option three is the preferred option of the basic option, in which the castable is a brown corundum mullite castable; the castable is a brown corundum mullite castable to extend the service life of the refractory material in the lime kiln.

[0011] Option 4 is the preferred option of the basic option. The spacing between two adjacent lifting bricks located in the preheating zone and calcining zone of the kiln body is 1000mm and 500mm respectively; the spacing between the lifting bricks in the preheating zone of the kiln body is set to 1000mm, which is convenient for lifting the limestone to a large height, lifting the powder particles between the materials and taking them away through the negative pressure of the system; the spacing between the lifting bricks in the calcining zone of the kiln body is set to 500mm, which is convenient for lifting the limestone to a small height, so that the limestone can roll evenly.

[0012] Scheme 5, a calcination method of a lime kiln for slowing down ring formation, comprising the following steps:

[0013] S1: First, the limestone is screened to obtain qualified limestone blocks;

[0014] S2: Convey qualified limestone blocks to the kiln preheating zone for preheating. As the kiln rotates, the limestone blocks in the kiln preheating zone are lifted up by the lifting bricks and turned over to fully contact with the high-temperature gas. At the same time, the limestone blocks roll from the kiln preheating zone to the kiln calcining zone.

[0015] S3: The limestone blocks entering the kiln calcining area are lifted up and turned by the lifting bricks. The high-temperature flame calcines and decomposes the limestone. At the same time, the limestone blocks roll from the kiln calcining area to the kiln discharging area.

[0016] S4: After the limestone blocks enter the discharging area, the active lime product is obtained and transported to the crushing system through the chain conveyor to be ground into active lime powder.

[0017] Through the above steps, the limestone is screened to ensure uniform particle size, which is convenient for uniform heating and improving calcination quality. In the preheating area, the limestone is fully contacted with the high-temperature gas by using the lifting bricks to achieve effective preheating in preparation for calcination. The lifting bricks in the calcining area ensure that the limestone is fully heated and decomposed, improve efficiency and quality, and make the limestone blocks evenly distributed to prevent local excessive temperature, thereby avoiding indirect ring formation.

[0018] Option 6 is a preferred option of Option 5. In S1, the particle size of the qualified limestone blocks is 20-35 mm. By limiting the particle size of the qualified limestone blocks to 20-35 mm, it is easy to ensure the uniformity of the calcined limestone blocks and reduce the difference in calcination effect caused by uneven particle size.

[0019] Option 7 is a preferred option of Option 5. In S2, the filling rate of the limestone blocks in the kiln body is 9%, and the temperature in the preheating zone of the kiln body is 900-1050°C. The filling rate and temperature of the limestone blocks in the kiln body are set to 9% and 900-1050°C, so that the limestone blocks have enough space in the kiln body for turning, contact and preliminary preheating, so as to prepare for subsequent calcination.

[0020] Option 8 is a preferred option of Option 5. In S3, the temperature of the kiln calcining zone is 1200-1350°C. Setting the temperature of the kiln calcining zone to 1200-1350°C facilitates the full reaction of the limestone blocks in the calcining zone and prevents the temperature from being too high or too low, which may lead to excessive sintering of the limestone blocks, accelerated ringing in the kiln body, or insufficient decomposition.

[0021] Option nine, which is the preferred option of option five, has a kiln speed of 400-800 r / min. Setting the kiln speed to 400-800 r / min facilitates the movement and reaction of limestone in the kiln to be in a suitable rhythm. When the speed is too high or too low, the limestone blocks are unevenly distributed in the kiln, there is too much or too little material in some local areas, and the temperature in some areas is too high, thereby slowing down the indirect formation of rings.

[0022] Scheme 10 is the preferred option of scheme 5. The limestone blocks stay in the preheating zone of the kiln for 120 to 200 minutes, in the calcining zone of the kiln for 60 to 120 minutes, and in the discharging zone of the kiln for 30 to 100 minutes. A reasonable residence time is set for each thermal zone in the kiln to facilitate the reaction standards at each stage and prevent excessive sintering, reduced activity or insufficient calcination of the limestone blocks due to excessive or insufficient residence time in each thermal zone in the kiln. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a three-dimensional diagram of a lime kiln for mitigating ring formation according to the present invention;

[0024] Figure 2 It is a right side view of a lime kiln for slowing down ring formation according to the present invention;

[0025] Figure 3 It is a structural schematic diagram of a material lifting brick in a lime kiln for alleviating ring formation according to the present invention;

[0026] Figure 4 It is a front view of a lime kiln for slowing down ring formation according to the present invention;

[0027] Figure 5 for Figure 4 The cross-sectional view at A~A in the middle;

[0028] Figure 6 The invention discloses a structural schematic diagram of a lime kiln for alleviating ringing when in use. DETAILED DESCRIPTION

[0029] The present invention is further described in detail below through specific embodiments:

[0030] The figure numerals in the drawings of the specification include: 1, kiln body; 2, lifting brick; 201, upper positioning groove; 202, lower positioning groove; 3, casting material; 4, preheating zone; 5, calcining zone; 6, discharge zone.

[0031] Example 1

[0032] like Figures 1 to 6 As shown: a lime kiln for slowing down ringing, comprising a kiln body 1, in which a plurality of lifting bricks 2 are welded, the thermal zone in the kiln body 1 is composed of a preheating zone 4, a calcining zone 5 and a discharging zone 6, the lifting bricks 2 are located in the preheating zone 4 and the calcining zone 5 of the kiln body, the spacing between two adjacent lifting bricks located in the preheating zone 4 and the calcining zone 5 of the kiln body is 1000 mm and 500 mm respectively, an upper positioning groove 201 and a lower positioning groove 202 are respectively provided on both sides of the lifting brick 2, and a castable 3 is filled between two adjacent lifting bricks 2, and the castable 3 is a castable made of brown corundum mullite.

[0033] The implementation method of this embodiment is as follows: when the lime kiln is needed, first, the limestone blocks enter the preheating zone 4 of the kiln body 1 for preheating. Under the rotation of the kiln body 1, the limestone blocks in the preheating zone 4 of the kiln body 1 are lifted up by the lifting bricks 2 and turned over to fully contact with the high-temperature gas. At the same time, the limestone blocks roll from the preheating zone 4 of the kiln body 1 to the calcining zone 5 of the kiln body 1. The limestone blocks entering the calcining zone 5 of the kiln body 1 are lifted up and turned over by the lifting bricks 2, and the high-temperature flame calcines and decomposes the limestone. At the same time, the limestone blocks roll from the calcining zone 5 of the kiln body 1 to the discharging zone 6 of the kiln body 1. After the limestone blocks enter the discharging zone 6, active lime products are obtained, which are transported to the crushing system through a chain conveyor and ground into active lime powder.

[0034] Example 2

[0035] like Figures 1 to 6 A calcination method of a lime kiln for slowing down ring formation comprises the following steps:

[0036] S1: First, the limestone is screened into qualified limestone blocks, wherein the particle size of the qualified limestone blocks is 30 mm;

[0037] S2: The qualified limestone blocks are transported to the preheating zone 4 of the kiln body 1 for preheating. Under the rotation of the kiln body 1, the limestone blocks in the preheating zone 4 of the kiln body 1 are lifted up by the lifting bricks 2 and turned over to fully contact with the high-temperature gas. At the same time, the limestone blocks roll from the preheating zone 4 of the kiln body 1 to the calcining zone 5 of the kiln body 1. The filling rate of the limestone blocks in the kiln body 1 is 9%, the temperature of the preheating zone of the kiln body 1 is 900°C, the residence time of the limestone blocks in the preheating zone 4 of the kiln body 1 is 200min, and the rotation speed of the kiln body 1 is 400r / min.

[0038] S3: The limestone blocks entering the calcining zone 5 of the kiln body 1 are lifted up and turned by the lifting bricks 2, and the high-temperature flame calcines and decomposes the limestone. At the same time, the limestone blocks roll from the calcining zone 5 of the kiln body 1 to the discharging zone 6 of the kiln body 1. The temperature of the calcining zone 5 of the kiln body 1 is 1100°C, and the residence time in the calcining zone 5 of the kiln body 1 is 120 minutes.

[0039] S4: After the limestone blocks enter the discharge area 6, the active lime products are obtained, which are transported to the crushing system through the chain conveyor and ground into active lime powder. Among them, they stay in the discharge area 6 of the kiln body 1 for 100 minutes.

[0040] By using the above parameters for calcination, it can be obtained that the ring-forming cycle of the lime kiln is 30 days, the final raw burning rate of calcium oxide in the limestone blocks is 78%, and the daily output is 500 tons (the daily output of the production line meets the standard of 800 tons), which does not meet the daily output standard of the production line, has a low output, and has a high energy consumption.

[0041] Example 3

[0042] like Figures 1 to 6A calcination method of a lime kiln for slowing down ring formation comprises the following steps:

[0043] S1: First, screen the limestone to find qualified limestone blocks, wherein the particle size of the qualified limestone blocks is 30 mm;

[0044] S2: conveying qualified limestone blocks to the preheating zone 4 of the kiln body 1 for preheating. Under the rotation of the kiln body 1, the limestone blocks in the preheating zone 4 of the kiln body 1 are lifted up by the lifting bricks 2 and turned over to fully contact with the high-temperature gas. At the same time, the limestone blocks roll from the preheating zone 4 of the kiln body 1 to the calcining zone 5 of the kiln body 1. The filling rate of the limestone blocks in the kiln body 1 is 9%, the temperature of the preheating zone 4 of the kiln body 1 is 1050°C, the residence time of the limestone blocks in the preheating zone 4 of the kiln body 1 is 120min, and the rotation speed of the kiln body 1 is 800r / min.

[0045] S3: The limestone blocks entering the calcining zone 5 of the kiln body 1 are lifted and turned by the lifting bricks 2, and the high-temperature flame calcines and decomposes the limestone. At the same time, the limestone blocks roll from the calcining zone 5 of the kiln body 1 to the discharging zone of the kiln body 1. The temperature of the calcining zone 5 of the kiln body 1 is 1350°C, and the residence time in the calcining zone 5 of the kiln body 1 is 60 minutes.

[0046] S4: After the limestone blocks enter the discharge area 6, the active lime products are obtained, which are transported to the crushing system through the chain conveyor and ground into active lime powder. Among them, they stay in the discharge area 6 of the kiln body 1 for 30 minutes.

[0047] By using the above parameters for calcination, the ring-forming period of the lime kiln is 50 days, the final raw burning rate of calcium oxide in the limestone blocks is 82%, and the daily output is 1,100 tons (the daily output of the production line is 800 tons), which meets the daily output standard of the production line. The output is relatively high, but the refractory material in the lime kiln falls off seriously and the energy consumption is relatively high.

[0048] Example 4

[0049] like Figures 1 to 6 A calcination method of a lime kiln for slowing down ring formation comprises the following steps:

[0050] S1: First, screen the limestone to find qualified limestone blocks, wherein the particle size of the qualified limestone blocks is 30 mm;

[0051] S2: conveying qualified limestone blocks to the preheating zone 4 of the kiln body 1 for preheating. Under the rotation of the kiln body 1, the limestone blocks in the preheating zone 4 of the kiln body 1 are lifted up by the lifting bricks 2 and turned over to fully contact with the high-temperature gas. At the same time, the limestone blocks roll from the preheating zone 4 of the kiln body 1 to the calcining zone 5 of the kiln body 1. The filling rate of the limestone blocks in the kiln body 1 is 9%, the temperature of the preheating zone 4 of the kiln body 1 is 950°C, the residence time of the limestone blocks in the preheating zone 4 of the kiln body 1 is 150min, and the rotation speed of the kiln body 1 is 600r / min.

[0052] S3: The limestone blocks entering the calcining zone 5 of the kiln body 1 are lifted and turned by the lifting bricks 2, and the high-temperature flame calcines and decomposes the limestone. At the same time, the limestone blocks roll from the calcining zone 5 of the kiln body 1 to the discharging zone 6 of the kiln body 1. The temperature of the calcining zone 5 of the kiln body 1 is 1250°C, and the residence time in the calcining zone 5 of the kiln body 1 is 90 minutes.

[0053] S4: After the limestone blocks enter the discharge area 6, the active lime products are obtained, which are transported to the crushing system through the chain conveyor and ground into active lime powder. Among them, they stay in the discharge area 6 of the kiln body 1 for 60 minutes.

[0054] By using the above parameters for calcination, the lime kiln ring formation period is 180 days, the final calcium oxide burning rate in the limestone blocks is 85%, the daily output is 900 tons (the daily output of the production line is 800 tons), which meets the daily output standard of the production line and reduces energy consumption by 1.5t / h.

[0055] In summary, by using the parameter control method in Example 4, the ring-forming cycle of the lime kiln is the longest, the raw burning rate of calcium oxide in the final limestone block is the highest, the daily output reaches the daily output standard of the production line, and the energy consumption is the lowest. It can be seen that by changing the movement form of the material inside the rotary kiln and adjusting the relevant residence time, temperature and rotation speed, the limestone can be fully contacted with the high-temperature gas, the decomposition of the limestone blocks can be improved, and the limestone blocks can be evenly distributed in the kiln body, the calcining zone temperature can be reduced, and the ring-forming speed can be slowed down.

[0056] The above is only an embodiment of the present invention, and the common knowledge such as the known specific structure and characteristics in the scheme is not described in detail here. It should be pointed out that for those skilled in the art, several deformations and improvements can be made without departing from the structure of the present invention, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A lime kiln for slowing down ring formation, characterized in that: The invention comprises a kiln body (1), wherein a plurality of lifting bricks (2) are arranged in the kiln body (1), the thermal zone in the kiln body (1) is composed of a preheating zone (4), a calcining zone (5) and a discharge zone (6), the lifting bricks (2) are located in the preheating zone (4) and the calcining zone (5) of the kiln body, and a casting material (3) is filled between two adjacent lifting bricks (2).

2. A lime kiln for slowing down ring formation according to claim 1, characterized in that: An upper positioning groove (201) and a lower positioning groove (202) are respectively provided on both sides of the lifting brick (2).

3. A lime kiln for mitigating ring formation according to claim 1, characterized in that: The castable (3) is a brown corundum mullite castable.

4. A lime kiln for mitigating ring formation according to claim 1, characterized in that: The distances between two adjacent lifting bricks (2) located in the kiln body preheating zone (4) and calcining zone (5) are 1000 mm and 500 mm respectively.

5. A calcining method for a lime kiln with slowed ring formation according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1: First, the limestone is screened to obtain qualified limestone blocks; S2: conveying qualified limestone blocks to the preheating zone (4) of the kiln body (1) for preheating. As the kiln body (1) rotates, the limestone blocks in the preheating zone (4) of the kiln body (1) are lifted up by the lifting bricks (2) and turned over to fully contact with the high-temperature gas. At the same time, the limestone blocks roll from the preheating zone (4) of the kiln body (1) to the calcining zone (5) of the kiln body (1); S3: The limestone blocks entering the calcining zone (5) of the kiln body (1) are lifted up and turned by the lifting bricks (2), and the high-temperature flames calcine and decompose the limestone. At the same time, the limestone blocks roll from the calcining zone (5) of the kiln body (1) to the discharging zone (6) of the kiln body (1); S4: After the limestone blocks enter the discharging area (6), the active lime product is obtained, which is transported to the crushing system through a chain conveyor and ground into active lime powder.

6. A calcining method for a lime kiln to slow down ring formation according to claim 5, characterized in that: In S1, the particle size of qualified limestone blocks is 20 to 35 mm.

7. A calcining method for a lime kiln to slow down ring formation according to claim 5, characterized in that: In S2, the filling rate of limestone blocks in the kiln body (1) is 9%, and the temperature of the preheating zone (4) of the kiln body (1) is 900-1050°C.

8. The calcining method of a lime kiln for slowing down ring formation according to claim 5, characterized in that: In S3, the temperature of the calcining zone (5) of the kiln body (1) is 1100-1350°C.

9. A calcining method for a lime kiln with reduced ringing according to claim 5, characterized in that: The rotation speed of the kiln body (1) is 400-800 r / min.

10. The calcining method of a lime kiln for slowing down ring formation according to claim 5, characterized in that: The limestone blocks stay in the preheating zone (4) of the kiln body (1) for 120 to 200 minutes, stay in the calcining zone (5) of the kiln body (1) for 60 to 120 minutes, and stay in the discharging zone (6) of the kiln body (1) for 30 to 100 minutes.