Sepiolite regenerated thermal insulation concrete

By combining sepiolite particles and regenerated fine aggregates in regenerated insulation concrete and optimizing the use of gas inducing agents, the problem of insufficient thermal and mechanical properties in the prior art is solved, and high efficiency, energy saving and good mechanical properties are achieved. Concrete meets the comprehensive performance needs of buildings.

CN118908662APending Publication Date: 2024-11-08HUNAN INSTITUTE OF ENGINEERING
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411056516.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing regenerated thermal insulation concrete has shortcomings in thermal and mechanical properties, and it is difficult to meet the needs of building energy conservation and emission reduction at the same time.

Method used

Using sepiolite particles and regenerated fine aggregates, a sepiolite regenerated insulation concrete is prepared by reasonably controlling the incorporation amount of sepiolite particles and regenerated fine aggregates, as well as the use of gas induction agents, and the preparation of a sepiolite regenerated insulation concrete for orthogonalization. The test is used to optimize the mix ratio to meet the requirements of both thermal and mechanical properties.

Benefits of technology

It has achieved regenerated thermal insulation concrete that is both efficient and energy-saving and has good mechanical properties. Through reasonable combination design, the thermal conductivity and compressive strength of the concrete are improved, meeting the thermal and mechanical properties requirements of the building.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908662A_ABST
    Figure CN118908662A_ABST
Patent Text Reader

Abstract

The invention discloses sepiolite regenerated thermal insulation concrete, and belongs to the technical field of concrete. Performance research of the recycled thermal insulation concrete is carried out on the basis of combination of sepiolite particles and recycled fine aggregate, aiming at the problem of poor thermal performance of common concrete and building energy conservation and emission reduction requirements, the recycled aggregate is used for replacing part of natural aggregate, a sepiolite inorganic thermal insulation material is doped, and a recycled thermal insulation concrete orthogonal test is carried out. The thermal performance and the mechanical performance of the building regenerated thermal insulation concrete are studied, and the structural regenerated thermal insulation concrete meeting the requirements of the thermal performance and the mechanical performance is obtained by strictly screening the mix proportion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of concrete, and in particular relates to a sepiolite recycled thermal insulation concrete. Background Art

[0002] Low-carbon concrete is an important engine to promote the development of the building materials industry, carrying the expectations and hopes of the whole society for low-carbon development. Therefore, the development of recycled thermal insulation concrete is particularly important and urgent.

[0003] At present, recycled concrete technology has made great progress and has been put into use in many practical projects. This technology has brought many revolutionary changes to the construction industry in the process of continuous evolution and improvement. The research results of developed countries in this field have fully proved the feasibility of its application technology, and it has gradually spread to more countries and regions. Compared with traditional concrete, recycled concrete has significant environmental advantages, reduces resource waste and carbon emissions, and contributes to the realization of sustainable development goals. In addition, the strength and durability of recycled concrete have also been improved, making it widely used in various engineering projects. With the continuous maturity of technology and the gradual acceptance of the market, recycled concrete is expected to play a greater role in the future construction field and bring more benefits to our society and environment.

[0004] However, in order to meet different needs, there is an urgent need for a structural recycled thermal insulation concrete that meets both thermal and mechanical performance requirements. Summary of the invention

[0005] In view of the above technical problems, the present invention proposes a sepiolite recycled thermal insulation concrete.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A sepiolite recycled thermal insulation concrete, based on basic concrete, replaces 25-100wt% of natural fine aggregate with recycled fine aggregate and at the same time, adds 5-20wt% of sepiolite particles as the recycled fine aggregate;

[0008] The basic concrete comprises the following components: cement, water, natural fine aggregate and water reducing agent.

[0009] Furthermore, the sepiolite recycled thermal insulation concrete also includes an air entraining agent added to the base concrete in an amount of 0.05-0.2% by mass of the base concrete.

[0010] Furthermore, the particle size of the recycled fine aggregate is 0.15-4.75 mm, the fineness modulus is 3.00, and the apparent density is 2300 kg / m 3 , crushing index is 19.3%, and micro powder content is 8.4%.

[0011] Furthermore, the particle size of the natural fine aggregate is 0.15-4.75 mm, the fineness modulus is 3.38, and the apparent density is 2583 kg / m 3 .

[0012] Furthermore, the density of the sepiolite particles is 1.099 g / m 3 , thermal conductivity is 0.178W / m·k, water absorption is 179.4%, and volume loss rate at 1MPa pressure is 0.001%.

[0013] Furthermore, the cement is P·O42.5 ordinary Portland cement.

[0014] Furthermore, the water reducing agent is a polycarboxylic acid high-efficiency water reducing agent, and the water reducing rate is 25%.

[0015] Furthermore, the base concrete includes the following components in parts by mass: 600 parts of cement, 330 parts of water, 1300 parts of natural fine aggregate and 2.2 parts of water reducing agent.

[0016] A preparation method of sepiolite recycled thermal insulation concrete comprises the following steps: mixing cement and water, adding sepiolite particles, stirring for 120 seconds, then adding natural fine aggregate and / or recycled fine aggregate, stirring for 120 seconds, and finally adding air entraining agent and water reducing agent, stirring again for 120 seconds, and curing to obtain sepiolite recycled thermal insulation concrete.

[0017] Compared with the prior art, the present invention has the following advantages and technical effects:

[0018] The invention obtains a structural recycled thermal insulation concrete that meets both thermal performance and mechanical performance requirements by reasonably controlling the amount of sepiolite particles added and the amount of replacement of recycled fine aggregates and the amount of air entraining agent added.

[0019] The present invention studies the performance of recycled thermal insulation concrete based on the combination of sepiolite particles and recycled fine aggregate. Aiming at the problem of poor thermal performance of ordinary concrete and the demand for building energy conservation and emission reduction, part of natural aggregate is replaced by recycled aggregate, sepiolite inorganic thermal insulation material is added, orthogonal test of recycled thermal insulation concrete is carried out, thermal performance and mechanical properties of building recycled thermal insulation concrete are studied, and a structural recycled thermal insulation concrete that meets both thermal performance and mechanical performance requirements is obtained by strictly screening the mix ratio. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0021] Figure 1Map the grading of natural river sand;

[0022] Figure 2 This is the gradation diagram of recycled fine aggregate;

[0023] Figure 3 This is a picture of sepiolite particles;

[0024] Figure 4 The process flow for preparing sepiolite recycled thermal insulation concrete;

[0025] Figure 5 The trend of the influence of various factors on thermal conductivity: (a) replacement rate of recycled fine aggregate, (b) amount of sepiolite particles, (c) amount of air-entraining agent;

[0026] Figure 6 The trends of the influence of various factors on compressive strength: (a) replacement rate of recycled fine aggregate, (b) amount of sepiolite particles, (c) amount of air-entraining agent;

[0027] Figure 7 The pores of SRIC9 at different scales; (a) 500 μm, (b) 200 μm;

[0028] Figure 8 This is the damage situation of SRIC9 test block;

[0029] Fig. 9 This is the cross-sectional view of the SRIC9 specimen after failure;

[0030] Fig.10 Pores at different scales in SRIC14; (a) 50 μm, (b) 500 μm;

[0031] Fig.11 The pores and cracks of SRIC18;

[0032] Fig.12 This is the cross-sectional view of the SRIC18 specimen after failure;

[0033] Fig.13 It is the hydration reaction of SRIC22 cement;

[0034] Fig.14 This is the cross-sectional view of the SRIC10 specimen after failure;

[0035] Fig.15 Cement hydration reaction around SRIC10 sepiolite particles; (a) 500μm, (b) 50μm. DETAILED DESCRIPTION

[0036] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0037] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0038] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0039] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0040] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0041] The "parts" described in the present invention, unless otherwise specified, refer to parts by mass.

[0042] The invention provides a sepiolite recycled thermal insulation concrete. On the basis of basic concrete, 25-100wt% of natural fine aggregate is replaced by recycled fine aggregate, and 5-20wt% of sepiolite particles of the recycled fine aggregate are added. The basic concrete comprises the following components: cement, water, natural fine aggregate and water reducing agent.

[0043] In some embodiments of the present invention, the sepiolite recycled thermal insulation concrete further comprises an air entraining agent added to the base concrete in an amount of 0.05-0.2% by mass of the base concrete.

[0044] In the following embodiments of the present invention, the natural fine aggregate is natural river sand produced by Xiangzhu Sand Field in Xiangtan City, with a particle size of 0.15-4.75 mm, a fineness modulus of 3.38, and an apparent density of 2583 kg / m 3 . Particle grading such as Figure 1 shown.

[0045] In the following embodiments of the present invention, the recycled fine aggregate is produced by a solid waste recycling company in Xiangtan, with a particle size of 0.15-4.75 mm, a fineness modulus of 3.00, and an apparent density of 2300 kg / m 3 , crushing index is 19.3%, and the micro powder content is 8.4%. Figure 2 shown.

[0046] In the following examples of the present invention, the cement used is P·O42.5 ordinary Portland cement produced by Hunan Hengyu Building Materials Co., Ltd. The physical properties are shown in Table 1, and the chemical composition is shown in Table 2.

[0047] Table 1 Physical properties of cement

[0048]

[0049] Table 2 Chemical composition of cement

[0050]

[0051] In the following examples of the present invention, the sepiolite particles used are sepiolite particles made from sepiolite powder by Xiangtan Yongbang Sepiolite Co., Ltd. (the production method is a conventional heating method, the particle size is 1-3 mm, the present invention will not repeat it, the sample morphology is shown in Figure 3 ), density is 1.099g / m 3 , thermal conductivity is 0.178W / m·k, water absorption is 179.4%, and volume loss rate at 1MPa pressure is 0.001%.

[0052] In the following embodiments of the present invention, the water reducer is a polycarboxylic acid high-efficiency water reducer produced by Hongxiang Building Admixture Factory, Laiyang City, Shandong Province, with a water reduction rate of 25%, and a polycarboxylic acid high-efficiency water reducer with a fineness greater than 0.315 mm accounting for less than 10%. Polycarboxylic acid high-efficiency water reducer is a high-performance water reducer and a cement dispersant used in cement concrete. It has a strong dispersing effect on cement particles and can comprehensively improve or improve various properties of concrete.

[0053] In the following embodiments of the present invention, the base concrete includes the following components in parts by mass: 600 parts of cement, 330 parts of water, 1300 parts of natural fine aggregate and 2.2 parts of water reducing agent.

[0054] The air entraining agent used in the present invention is a concrete air entraining agent (high-purity type of Huiba concrete air entraining agent) produced by Hongxiang Building Admixture Factory in Laiyang City, Shandong Province. Concrete air entraining agent can greatly improve the workability and pumpability of concrete and improve its durability such as anti-seepage and anti-freeze. It can also effectively prevent the secondary adsorption of cement in concrete and reduce the loss of concrete slump over time. Due to the high water reduction rate, the use of water reducer can be greatly reduced, saving application costs and increasing economic benefits.

[0055] A preparation method of sepiolite recycled thermal insulation concrete comprises the following steps: mixing cement and water, adding sepiolite particles, stirring for 120 seconds, then adding natural fine aggregate and / or recycled fine aggregate, stirring for 120 seconds, and finally adding air entraining agent and water reducing agent, stirring again for 120 seconds, and curing to obtain sepiolite recycled thermal insulation concrete.

[0056] The technical solution of the present invention is further illustrated by the following embodiments.

[0057] Example 1

[0058] The benchmark mix ratio of sepiolite recycled thermal insulation concrete was tested. The benchmark mix ratio was calculated based on the 150mm×150mm×150mm test block by referring to the mix ratio proposed in "JGJ55-2011 Ordinary Concrete Mix Design Code" and "JGJT443-2018 Recycled Concrete Structure Technical Standard", and the benchmark mix ratio is shown in Table 3.

[0059] Table 3 Basic mix ratio

[0060]

[0061] The test blocks were cured according to GB / T50081-2002 Standard for Test Methods of Physical and Mechanical Properties of Concrete. The prepared blocks were placed in a SHBY-40B CNC cement concrete standard curing box with a set temperature of 20°C and a relative humidity of 95%. The curing ages of the prepared test blocks were 7d, 14d and 28d.

[0062] The basic concrete of this experiment includes the following components: cement, water, natural fine aggregate and water reducing agent. Under this premise, A (recycled fine aggregate replacement rate, which refers to the amount of recycled fine aggregate replacing natural fine aggregate), B (sepiolite particle dosage, which refers to the percentage of natural fine aggregate mass) and C (air entraining agent dosage, which refers to the percentage of base concrete mass) are used as the factors of the orthogonal test of sepiolite recycled thermal insulation concrete. In order to make the test data more sufficient, each factor takes five levels and conducts equal-level orthogonal test design. The factor level table is shown in Table 4.

[0063] The preparation method of sepiolite recycled thermal insulation concrete is as follows: after mixing cement and water, add sepiolite particles, stir for 120 seconds, then add natural fine aggregate and / or recycled fine aggregate, stir for 120 seconds, finally add air entraining agent and water reducing agent, stir again for 120 seconds, put into a test block mold of 100mm×100mm×100mm (8 test blocks are made in each group, totaling 25 groups), and cure at a temperature of 20°C and a relative humidity of 95% for 7 days, 14 days and 28 days to obtain sepiolite recycled thermal insulation concrete (preparation method see Figure 4 ).

[0064] During the trial period, the mold used needs to be brushed with mold release oil, and a piece of paper should be pasted on the air holes at the bottom of the mold to ensure that the air holes are not blocked by the mixture during demoulding. Pour the mixture into the mold and place it on the concrete vibration table for compaction. During the vibration process, use a scraper to scrape off the mixture overflowing from the surface and smooth it. After compaction, place the mixture and the mold in a cool room for natural curing for one day before demoulding.

[0065] Table 4 Orthogonal test level table

[0066]

[0067] This experiment uses a three-factor five-level orthogonal test, without considering the interaction, so the orthogonal table that meets this experiment is L 25 (5 6 ). Since the number of factors is 3, the orthogonal test table is based on L 25 (5 6 ) The first three columns are designed. The orthogonal table is shown in Table 5.

[0068] Table 5 Orthogonal test table of sepiolite recycled thermal insulation concrete

[0069]

[0070]

[0071] Range analysis: Range analysis is simple to operate and can determine the degree of influence of factors. The larger the range, the greater the influence of the factor on the results of the orthogonal test; conversely, the smaller the range, the smaller the influence of the factor on the results of the orthogonal test.

[0072] K i : Represents the sum of the test results corresponding to the level number i in any column.

[0073] k i :k i =K i / s, s is the number of times a level appears in any column, k i It represents the arithmetic mean of the test results corresponding to the level number i in any column.

[0074] R: R is the range, R = max{K}-min{K} in any column.

[0075] By comparing the range of each factor and using the comprehensive balance method, the analysis results of each indicator are comprehensively compared and analyzed to obtain the optimal solution.

[0076] ANOVA: ANOVA is a statistical method used to compare whether the means of two or more groups are significantly different. The basic idea of ​​ANOVA is that if the difference between groups is greater than the difference within the groups, then the means between the groups can be considered to be significantly different.

[0077] The basic steps of ANOVA for orthogonal experiments are as follows:

[0078] (1) According to the design table of the orthogonal experiment, calculate the average effect of each factor and interaction, that is, the average experimental results at each level.

[0079] (2) Calculate the total sum of squares (S T ), which is the sum of the squares of the differences between all test results and the grand mean.

[0080]

[0081] (3) Calculate the sum of squares of factors and interactions (SSA), that is, the sum of the squares of the differences between the average effects of each factor and interaction and the overall mean, multiplied by the corresponding degrees of freedom.

[0082]

[0083] A——represents factor, different factors correspond to different letters.

[0084] K pj ——Represents the average of r experimental results at the pth (p=1, 2, 3,…, m) level of A.

[0085] (4) Calculate the sum of squared errors (SSE), which is the total sum of squares minus the sum of squares of each factor and interaction.

[0086] S e =S T -The sum of the squared deviations of each factor

[0087] (5) Calculate the mean square estimate (MSA) of each factor and interaction, which is the sum of the squares of each factor and interaction divided by the corresponding degrees of freedom.

[0088]

[0089] A represents the same content as above.

[0090] (6) Calculate the mean square error (MSE), which is the sum of squared errors divided by the corresponding degrees of freedom.

[0091]

[0092] (7) Calculate the F value (FA) of each factor and interaction, that is, the mean square of each factor and interaction divided by the error mean square.

[0093]

[0094] A represents the same content as above.

[0095] (8) Based on the given significance level (α) and degrees of freedom, the critical F value (Fc) is obtained by looking up the table.

[0096] (9) Compare the F values ​​of each factor and interaction with the critical F value. If F A >F c , then the factor or interaction is considered to have a significant effect on the test results, otherwise it is considered to have no significant effect.

[0097] (10) For factors or interactions with significant influence, further analyze their effect sizes, rank them according to effect sizes, and determine the optimal level combination.

[0098] The orthogonal test data of the present invention uses Minitab 21 to create Taguchi design, analyze Taguchi design, and perform general linear model variance analysis. Minitab 21 is a powerful statistical analysis tool that makes orthogonal test design and statistical analysis more convenient and efficient, helps to better understand the test data, make wise decisions, and ultimately optimize research results.

[0099] Test method:

[0100] 1. Compressive strength test: The compressive strength test of the test block refers to the "GB / T50081-2002 Standard for Test Methods for Physical and Mechanical Properties of Concrete". The test blocks cured to the corresponding age are tested for compressive strength using a hydraulic universal testing machine, and the load loading speed is 0.4MPa / s.

[0101] The compressive strength of the cube is calculated according to the following formula:

[0102]

[0103] Where: f cc ——Compressive strength of concrete cube specimen (MPa), the calculation result should be accurate to 0.1MPa;

[0104] F——Specimen failure load (N)

[0105] A——Test piece pressure bearing area (mm 2 ).

[0106] 2. Thermal conductivity test: According to GB / T32064-2015 Transient Plane Heat Source Test Method for Thermal Conductivity and Thermal Diffusivity of Building Materials, use HS-DR-5 transient thermal conductivity meter to test thermal conductivity.

[0107] The thermal conductivity is calculated according to the following formula:

[0108]

[0109]

[0110] ΔT s (τ)——the function of the sample surface temperature increment during the test as a function of τ, K;

[0111] P 0 ——Output power of the probe, W;

[0112] r——The outermost radius of the double helix structure of the probe, mm;

[0113] λ——thermal conductivity of sample, W / (m·K);

[0114] D(τ) – dimensionless characteristic time function;

[0115] t——test time, s;

[0116] t c ——correction time, s;

[0117] a——thermal diffusivity of the sample, mm 2 / s;

[0118] m——the total number of rings in the double helix structure of the probe;

[0119] σ——integral variable of dimensionless characteristic time function;

[0120] l 1 , l 2 ——a summation variable not greater than the total number of rings in the double helix structure;

[0121] J 0 ——Zero-order modified Seer function.

[0122] 3. SEM scanning: Use SU3500 scanning electron microscope for microscopic analysis.

[0123] Result analysis:

[0124] 1. Analysis of factors affecting thermal conductivity

[0125] The compressive strength and thermal conductivity of the orthogonal test of sepiolite recycled thermal insulation concrete are shown in Table 6. The range analysis table of thermal conductivity is shown in Table 7, and the variance analysis of thermal conductivity is shown in Table 8.

[0126] Table 6 Orthogonal and control test table and test results

[0127]

[0128]

[0129] Table 7 Thermal conductivity range analysis table

[0130]

[0131] Table 8 Thermal conductivity variance analysis table

[0132]

[0133]

[0134] Note: “**” indicates a highly significant factor, “*” indicates a significant factor, and “—” indicates an insignificant factor.

[0135] From Table 7, we can see that the range of the three factors is C>B>A, that is, the influence of each factor on the thermal conductivity is: C (air entraining agent dosage)>B (sepiolite particle dosage)>A (recycled fine aggregate replacement rate). From Table 8, we can see that the air entraining agent dosage has a significant effect on the thermal conductivity, while the sepiolite particle dosage and the recycled fine aggregate replacement rate have no significant effect on the thermal conductivity. Figure 5 It can be seen that the thermal conductivity decreases with the increase of the air entraining agent content. The thermal conductivity of the SRIC with 0.2% air entraining agent is reduced by 36.5% compared with the SRIC with 0% air entraining agent. This is because the air entraining agent introduces a large number of stable and closed bubbles (such as Figure 7 The thermal conductivity of air is low, which reduces the overall thermal conductivity of concrete.

[0136] When the content of sepiolite particles is 5%, the thermal conductivity of SRIC is reduced by 15.1% compared with the thermal conductivity of SRIC with 0% sepiolite particles. This is because when the content of sepiolite particles is 5%, the sepiolite particles have little effect on the free water of SRIC mixture, and due to the pre-wetting treatment of sepiolite particles, the water in the sepiolite particles participates in the cement hydration reaction during the curing stage, which increases the water-cement ratio of SRIC, resulting in more pores in the cement hydration reaction, which together with the sepiolite particles reduce the thermal conductivity of SRIC; when the content of sepiolite particles is 10%, the thermal conductivity of SRIC is increased by 10.7% compared with the thermal conductivity of SRIC with 5% sepiolite particles, and when the content of sepiolite particles is greater than 10%, the thermal conductivity of SRIC decreases with the increase of the content of sepiolite particles. The increase in the amount of sepiolite particles makes the sepiolite particles absorb some free water during the mixing process of the SRIC mixture, thereby reducing the effective water-cement ratio, which reduces the porosity of the cement during the hydration reaction, increases the density of SRIC and thus increases the thermal conductivity. Since the thermal conductivity of sepiolite particles is low, when the amount of sepiolite particles is increased, the synergistic effect of sepiolite particles, recycled aggregate and air entraining agent leads to a lower thermal conductivity of SRIC.

[0137] When the replacement rate of recycled fine aggregate is less than 75%, the thermal conductivity decreases with the increase of the replacement rate of recycled aggregate, and the reduction gradually decreases. This is because the porosity of recycled aggregate is high. As the replacement rate of recycled fine aggregate increases, the internal porosity of SRIC increases, resulting in a decrease in thermal conductivity. When the replacement rate of recycled fine aggregate reaches 100%, the thermal conductivity increases. This is because the recycled fine aggregate used in this test has stronger water absorption than natural sand. When the replacement rate of recycled fine aggregate is 100%, the recycled aggregate absorbs part of the water during the mixing process of SRIC mixture, reducing the effective water-cement ratio, which reduces the porosity of cement during the hydration reaction and increases the dry-wet apparent density, resulting in an increase in thermal conductivity.

[0138] 2. Analysis of factors affecting compressive strength

[0139] The range analysis table of 28d compressive strength is shown in Table 9.

[0140] Table 9 Compressive strength range analysis table

[0141]

[0142] The variance analysis table of 28d compressive strength is shown in Table 10.

[0143] Table 10 Variance analysis table of compressive strength

[0144]

[0145] Note: “**” indicates a highly significant factor, “*” indicates a significant factor, and “—” indicates an insignificant factor.

[0146] As shown in Table 9, Ki is the sum of the test results corresponding to the level number i in any column, and R is the range. As shown in Table 10, RC>RA>RB, the influence of each factor on the 28d compressive strength is ranked as follows: C (amount of air entraining agent)>B (amount of sepiolite particles)>A (recycled fine aggregate replacement rate), so the effect of air entraining agent on the 28d compressive strength is highly significant, and the effect of the replacement rate of recycled fine aggregate and the amount of sepiolite particles on the 28d compressive strength is generally significant.

[0147] Analysis of the compressive strength test results shows that the air entraining agent causes a large number of bubbles to form in the mixing process of the sepiolite recycled thermal insulation concrete. Before and after the final setting of the sepiolite recycled thermal insulation concrete, these bubbles form a large number of internal pores, which seriously affect the structural stability of the sepiolite recycled thermal insulation concrete, resulting in a significant decrease in strength, so that when calculating the extreme difference, the extreme differences of the two factors, sepiolite particle dosage and recycled fine aggregate replacement rate, are relatively low.

[0148] Figure 6 is the influence trend of each factor on compressive strength. Figure 6 It can be seen that the compressive strength of SRIC at 7d, 14d, and 28d decreases with the increase of the amount of air-entraining agent. This is because the air-entraining agent will produce a large number of bubbles during the mixing process of concrete, and these bubbles will gradually form pore structures (such as Figure 7 As shown in Figure 2). According to the pore structure classification, it is divided into harmless pore level (pore size <200μm), less harmful pore level (pore size = 200-500μm), harmful pore level (pore size = 500-2000μm) and more harmful pore level (pore size > 2000μm). Too much air entraining agent causes a large number of bubbles to collide with each other and squeeze cement particles to form larger bubbles. These bubbles cause a large number of pores above the harmful pore level to form inside the SRIC (such as Figure 8 , Fig. 9 ), which greatly affects the compressive strength.

[0149] When the replacement rate of recycled fine aggregate is less than 75%, the 7d, 14d, and 28d compressive strengths decrease with the increase of the replacement rate of recycled fine aggregate. When the replacement rate of recycled fine aggregate is 75%, the compressive strength reaches the lowest point, decreasing by 29.8%, 34.8%, and 28.9%, respectively. This is because the main component of recycled aggregate is broken concrete particles, and its strength is much lower than that of natural aggregate. In addition, due to the high water-binder ratio, the cement hydration reaction produces more pores (such as Fig.10 As shown, the replacement rate of recycled fine aggregate is 50%; Fig.11 and Fig.12As shown in the figure, the replacement rate of recycled fine aggregate is 75%), and the strength is reduced due to the influence of multiple unfavorable factors.

[0150] When the replacement rate of recycled fine aggregate reaches 100%, the compressive strengths at 7d, 14d and 28d have an upward trend, and are all higher than the SRIC at each age with a replacement rate of 25% recycled fine aggregate. Compared with the compressive strength at a replacement rate of 75%, the compressive strengths at 7d, 14d and 28d increase by 27.4%, 33.8% and 29.6%, respectively. On the one hand, this is because the recycled aggregate has a high water absorption rate. The recycled thermal insulation concrete with a water-binder ratio of 0.55 absorbs free effective water, which reduces the effective water-binder ratio and increases the bonding ability between the recycled aggregate and the cement paste. On the other hand, the recycled aggregate contains a small amount of unhydrated cement particles, which continue to undergo hydration reactions during the curing process (such as Fig.13 As shown, the replacement rate of recycled fine aggregate is 100%), which is equivalent to increasing the amount of SRIC cement, which is beneficial to improving the compressive strength.

[0151] The SRIC compressive strength at 7d, 14d and 28d decreased with the increase of sepiolite particle dosage before 15%. Compared with 0% sepiolite particle dosage, the SRIC compressive strength at the lowest point of 15% sepiolite particle dosage decreased by 39.1%, 41.6% and 32.0% respectively. This is because the sepiolite particles are large in size, low in strength and low in density. The sepiolite particles are evenly dispersed in the concrete, which weakens the connection between the sepiolite particles and the aggregate, forming weak areas, which have an adverse effect on the compressive strength. When the sepiolite particle dosage reaches 20%, the SRIC strength increases by 20.0%, 21.6% and 11.5% at 7d, 14d and 28d respectively compared with the SRIC strength of 15% sepiolite particles. On the one hand, when the amount of sepiolite particles is too high, although the sepiolite particles are pre-wetted, they still absorb part of the free water of the SRIC mixture during the mixing process of the SRIC mixture, reducing the effective water-binder ratio in the transition zone between the sepiolite particles and the mortar interface, which increases the compressive strength of the SRIC mixture (e.g. Fig.14 ); on the other hand, due to the low strength of sepiolite particles themselves, the sepiolite particles rub against the inner wall of the mixer during the mixing of the SRIC mixture, causing some of the sepiolite particles to break and form sepiolite powder. The sepiolite powder has strong water absorption. A certain amount of sepiolite powder can reduce the free water between cement particles, reduce the effective water-binder ratio, and increase the strength of the mortar, thereby improving the overall strength of the SRIC. Its hydration products such as Fig.15 As shown (SRIC10 is the content of sepiolite particles 20%).

[0152] 3. Comprehensive analysis

[0153] From Table 7 and Table 8, we can see that the optimal scheme for compressive strength is A1B1C1, and from Table 7 and Table 8, we can see that the optimal scheme for thermal conductivity is A4B5C5. Fig. 9 and Fig.10 It can be obtained that the higher the compressive strength, the higher the thermal conductivity; similarly, the lower the compressive strength, the lower the thermal conductivity. In order to explore the mix ratio with the best comprehensive performance, that is, the mix ratio with low thermal conductivity under the premise that the compressive strength meets the standard, the following analysis is carried out in combination with the data in Tables 9 and 10: the group with compressive strength greater than 20MPa, namely SRIC1, SRIC10, and SRIC22, is screened out, and the compressive strength is ranked in order of SRIC1 (29.4MPa) > SRIC10 (25.3MPa) > SRIC22 (21.05MPa), and the thermal conductivity is ranked in order of SRIC1 (1.0010) > SRIC22 (0.5202) > SRIC10 (0.4247). Taking all factors into consideration, the best performance mix ratio is SRIC10.

[0154] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A sepiolite recycled thermal insulation concrete, characterized in that: On the basis of the base concrete, 25-100 wt% of the natural fine aggregate is replaced by the same mass of recycled fine aggregate, and 5-20 wt% of the mass of the recycled fine aggregate is mixed with sepiolite particles; The basic concrete comprises the following components: cement, water, natural fine aggregate and water reducing agent.

2. The sepiolite recycled thermal insulation concrete according to claim 1, characterized in that: The method also includes adding an air entraining agent to the base concrete, wherein the amount of the air entraining agent added is 0.05-0.2% of the mass of the base concrete.

3. The sepiolite recycled thermal insulation concrete according to claim 1 or 2, characterized in that: The particle size of the recycled fine aggregate is 0.15-4.75 mm, the fineness modulus is 3.00, and the apparent density is 2300 kg / m 3 , crushing index is 19.3%, and micro powder content is 8.4%.

4. The sepiolite recycled thermal insulation concrete according to claim 1 or 2, characterized in that: The particle size of the natural fine aggregate is 0.15-4.75 mm, the fineness modulus is 3.38, and the apparent density is 2583 kg / m 3 .

5. The sepiolite recycled thermal insulation concrete according to claim 1 or 2, characterized in that: The density of the sepiolite particles is 1.099 g / m 3 , thermal conductivity is 0.178W / m·k, water absorption is 179.4%, and volume loss rate at 1MPa pressure is 0.001%.

6. The sepiolite recycled thermal insulation concrete according to claim 1 or 2, characterized in that: The cement is P·O42.5 ordinary Portland cement.

7. The sepiolite recycled thermal insulation concrete according to claim 1 or 2, characterized in that: The water reducing agent is a polycarboxylic acid high efficiency water reducing agent, and the water reducing rate is 25%.

8. The sepiolite recycled thermal insulation concrete according to claim 1 or 2, characterized in that: The base concrete includes the following components in parts by mass: 600 parts of cement, 330 parts of water, 1300 parts of natural fine aggregate and 2.2 parts of water reducing agent.

9. A method for preparing the sepiolite recycled thermal insulation concrete according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: mixing cement and water, adding sepiolite particles, stirring for 120 seconds, then adding natural fine aggregate and / or recycled fine aggregate, stirring for 120 seconds, and finally adding air entraining agent and water reducing agent, stirring again for 120 seconds, and curing to obtain sepiolite recycled thermal insulation concrete.

Citation Information

Patent Citations

  • Sepiolite aerated concrete block and preparation process thereof

    CN112250467A

  • Freeze-thaw resistant recycled concrete

    CN117534417A