Lingnan grey sculpture material, preparation method thereof, grey sculpture product and manufacturing process of grey sculpture product

By improving Lingnan gray plastic materials and processes, using grassroots ash, paper-rod ash, pounding ash and other materials and 3D printing technology, the problems of the durability and construction technology inheritance of traditional gray plastic materials have been solved, and higher durability and beauty have been achieved and improve construction efficiency.

CN118908681AActive Publication Date: 2024-11-08GUANGZHOU HOUSES DEV CONSTR

Patent Information

Application Number
CN202410958429.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

Traditional Lingnan gray plastic materials and processes have problems with durability and aesthetics, resulting in shortening of their shelf life and difficulty in inheriting construction techniques.

Method used

Improved materials such as grassroots ash, paper-rod ash, pounded ash or colored ash, combined with fermentation and 3D printing technology, optimize the production process of gray plastic products, and improve crack resistance and construction efficiency.

Benefits of technology

It significantly extends the service life of gray plastic, reduces construction difficulty, improves durability and aesthetics, and promotes the inheritance and development of gray plastic technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908681A_ABST
    Figure CN118908681A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of building decoration and cultural relic protection, in particular to a Lingnan grey plastic material, a preparation method thereof, a grey plastic product and a manufacturing process. The grey plastic material comprises at least one of grass root ash, paper strip ash, pounding ash or color ash, dry straw and jade button paper are added into the grey plastic material, the preparation process is combined for improvement, the crack resistance and toughness of the grey plastic are remarkably improved, and then the service life of the grey plastic is prolonged; the improved grey plastic material reduces the construction difficulty of a grey plastic coating process, and further combines with 3D printing to manufacture a grey plastic framework, so that the construction efficiency can be greatly improved, the yield can be improved, and the inheritance and development of the grey plastic process are facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building decoration and cultural relic protection, and in particular to a Lingnan gray plastic material and a preparation method thereof, a gray plastic product and a manufacturing process thereof. Background Art

[0002] Gray sculpture is a traditional architectural decoration originating from the Lingnan region, carrying a profound historical and cultural heritage. However, in the long-term use process, traditional gray sculpture materials and craftsmanship have shown some problems, which not only affect the durability and aesthetics of gray sculpture, but also hinder the inheritance and development of gray sculpture.

[0003] In terms of material durability, traditional plaster plastics are mainly composed of lime and paper tendons. After being exposed to the natural environment for a long time, their surfaces are prone to fading and cracking, which seriously affects the shelf life and ornamental value of the plaster plastics.

[0004] In terms of craft inheritance and development, the traditional plaster plastic product process is complex and delicate, and requires high construction skills, which seriously affects the inheritance and development of plaster plastic skills. Summary of the invention

[0005] In response to the problems existing in the materials and production techniques of traditional Lingnan plaster sculptures, the traditional Lingnan plaster sculpture materials are improved, and on this basis the production techniques of plaster sculpture products are also improved, which effectively enhances the durability of plaster sculptures and promotes the inheritance and development of the plaster sculpture technique.

[0006] The first aspect of the present invention provides a method for preparing a Lingnan ash plastic material, wherein the ash plastic material comprises at least one of grass root ash, paper tendon ash, pounded ash, or colored ash.

[0007] The preparation method of the grass tendon ash comprises the following steps: firstly, 10-30 parts by weight of quicklime and 3-10 parts by weight of rice straw are uniformly mixed, then 0.3-2 parts by weight of hemp silk are added and fully stirred, then the mixture is sealed, soaked and fermented, the fermentation time is 3-5 days, the mixture should be turned over every 8 hours during the fermentation period, after the fermentation is completed, the mixture is dried, and then ground or crushed to obtain the grass tendon ash;

[0008] The preparation method of the paper tendon ash comprises the following steps: firstly, 40-60 parts by weight of lime paste, 5-15 parts by weight of water, 3-10 parts by weight of glutinous rice paste, and 0.5-2 parts by weight of jade button paper are mixed and stirred evenly, and then sealed, soaked and fermented for 2-4 days, and the mixture is turned over every 8 hours. After the fermentation is completed, the mixture is dried, and then ground or crushed to obtain the grass tendon ash;

[0009] The preparation method of pounded ash comprises the following steps: evenly mixing 30-50 parts by weight of grass tendon ash prepared by the preparation method, 20-30 parts by weight of paper tendon ash prepared by the preparation method, 1-3 parts by weight of quicklime, 1-3 parts by weight of brown sugar, 0.5-2 parts by weight of glutinous rice flour, and 0.5-2 parts by weight of lime oil, and repeatedly beating the mixture with a pestle for 30-60 minutes until the mixture becomes smooth and sticky;

[0010] The method for preparing the colored ash comprises the steps of: mixing the pounded ash prepared by the above-mentioned preparation method with the pigment and stirring for 10-20 minutes, and then standing for 12-24 hours.

[0011] Preferably, the temperature of the sealed fermentation of the straw ash or paper ash is 20-30° C. and the humidity is 60-80%.

[0012] Preferably, the quicklime in the grass ash is a superior grade or higher calcium quicklime, the CaO content in the calcium quicklime is above 85% (by weight), and the fineness is above 60 mesh. The superior grade calcium quicklime has a higher content of calcium oxide (CaO), contains more effective ingredients, and can provide stronger bonding force and better use effect.

[0013] Preferably, in the glutinous rice paste in the paper tendon ash, the weight ratio of water to glutinous rice flour is 1:2 to 1:3, and the bonding performance is good.

[0014] Preferably, the mass ratio of calcium oxide to water in the lime paste in the paper tendon ash is between 1:3 and 1:4.

[0015] Preferably, the lime oil in the pounded lime is also called "tung oil lime", which is obtained by mixing slaked lime and tung oil in a mass ratio of 3:1.

[0016] Preparation process: Filter slaked lime (Ca(OH)2) through a fine sieve to remove impurities and unburned limestone particles. Tung oil also needs to be filtered through gauze to remove possible impurities and sediments. Then mix the filtered slaked lime and tung oil in a mass ratio of 3:1 to obtain the product.

[0017] The quicklime in the pounded lime is calcium quicklime of superior grade or above, the content of CaO in the calcium quicklime is above 85%, and the fineness is above 60 meshes.

[0018] The second aspect of the present invention also provides Lingnan gray plastic material prepared by the above preparation method.

[0019] The third aspect of the present invention also provides a plaster plastic product made from the above plaster plastic material.

[0020] The fourth aspect of the present invention further provides a process for producing the gray plastic product, comprising the following steps:

[0021] Concept and design patterns: Based on the architectural space and decoration requirements, combined with the pattern's theme, layout, color matching and cultural implication, conceive and design suitable gray sculpture patterns;

[0022] Measurement and design: According to the design pattern, the building parts are accurately measured, and the design pattern is appropriately adjusted and optimized according to the measurement results. Ensure that the plaster plastic can fit the installation position;

[0023] Sketching: Sketching the plastering sketch of the building parts according to the design pattern and measurement results. Providing guidance for the subsequent skeleton construction and plastering work;

[0024] Tie-up the frame: According to the traditional craftsmanship and the sketch, steel nails can be driven into the corresponding parts of the building, and the copper wire can be used to accurately and firmly tie up the frame according to the sketch;

[0025] Wrapping the ash: Wrap the pounded ash layer by layer on the modeling frame, with each layer thickness not exceeding 3 cm and a time interval of not less than 24 hours, until the ash sculpture embryo is completed;

[0026] Coloring: After the gray plastic embryo is stable, use the gray color to color it according to the design pattern. Wait 4 hours after each layer of color;

[0027] Outlining: After coloring is completed, use the gray to outline the gray sculpture contours and detail lines;

[0028] Sealing and maintenance: Waterproof and sun-proof within 5 days after the gray plastic is completed.

[0029] By optimizing the materials, there is no need to first apply straw ash to the base and then paper ash to press the surface, but the initial blank can be directly made by pounding ash.

[0030] Furthermore, 3D printing can also be used to make the modeling skeleton, and the corresponding gray plastic product manufacturing process includes the following steps:

[0031] Measurement and modeling: According to the design pattern, the building parts are accurately measured, and the design pattern is appropriately adjusted and optimized according to the measurement results, and then the gray modeling skeleton is three-dimensionally modeled using 3DSMAX technology; preferably, ABAQUS finite element analysis software is used to perform mechanical analysis on the three-dimensional model of the modeling skeleton to ensure that it has sufficient bearing capacity and stability after printing.

[0032] Printing the modeling skeleton: Import the gray modeling skeleton three-dimensional model into the 3D printer, select aluminum alloy material for layer-by-layer printing, and produce the modeling skeleton.

[0033] In a preferred embodiment, the aluminum alloy material contains the following weight percentages of metal elements: 90% aluminum, 5% magnesium, 3% silicon, 1% copper and 1% zinc. The aluminum alloy material has good lightweight and welding properties, with a density of about 2.7 g / cm3, which is much lower than traditional steel and is easy to install and fix.

[0034] In a preferred embodiment, the printing speed is adjusted to a stacking height of no more than 5mm per minute to ensure that the aluminum alloy material can be stacked smoothly and reduce thermal stress; the printing temperature is controlled between 400-450℃ to ensure that the aluminum alloy material maintains good fluidity and bonding during the printing process; the layer thickness is set to 0.2mm to improve printing accuracy and reduce printing time; the filling density is optimized to 90% to ensure that the printed skeleton has sufficient strength and stability. After the printing process is optimized, the tensile strength of the modeling skeleton reaches 360MPa, the yield strength reaches 280MPa, and the elongation reaches 9%, which can withstand various forces and deformations in the gray plastic production process.

[0035] Install the modeling frame: Fix the printed modeling frame to the building.

[0036] Preferably, angle steel can be implanted in corresponding building locations and fixed to the modeling frame by bolts.

[0037] Preferably, a support structure can be implanted in a corresponding building site, the support structure penetrates into the modeling frame and is welded to the modeling frame so as to better support the modeling frame.

[0038] Lime wrapping: Wrap the pounded ash layer by layer on the modeling frame, with each layer thickness not exceeding 3 cm and a time interval of not less than 24 hours, until the ash sculpture embryo is completed.

[0039] Coloring: After the gray plastic embryo is stable, it is colored with the gray according to the design pattern. It takes 4 hours to wait after each layer of color.

[0040] Outlining lines: After coloring is completed, use the above-mentioned gray to outline the gray sculpture contours and detail lines.

[0041] Sealing and maintenance: Waterproof and sun-proof within 5 days after the gray plastic is completed.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] The present invention significantly improves the crack resistance and toughness of the gray plastic by adding dry straw and jade button paper to the gray plastic material and improving the preparation process, thereby extending its service life; the improved gray plastic material reduces the construction difficulty of the gray packaging process, and further combines 3D printing to make a gray plastic skeleton, which can greatly improve the construction efficiency and the yield rate, which is conducive to the inheritance and development of the gray plastic process. The present invention improves the durability, aesthetics and ease of construction of the gray plastic as a whole. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 This is a process flow chart of manufacturing a gray plastic product according to Example 2 of the present invention;

[0045] Figure 2 This is a process flow chart of manufacturing a gray plastic product according to Embodiment 3 of the present invention;

[0046] Figure 3 This is one of the views of the connection structure of the gray plastic product modeling skeleton according to an embodiment of the present invention;

[0047] Figure 4 This is the second view of the connection structure of the gray plastic product modeling skeleton according to the embodiment of the present invention;

[0048] Figure 5 This is the third view of the connection structure of the gray plastic product modeling skeleton according to the embodiment of the present invention;

[0049] Figure 6 This is the fourth view of the connection structure of the gray plastic product modeling skeleton according to an embodiment of the present invention. DETAILED DESCRIPTION

[0050] The present invention provides a Lingnan lime plastic material, which is mainly composed of lime and paper tendons and is prone to fading, peeling and the like after being exposed to the natural environment for a long time. The lime plastic material includes at least one of grass root lime, paper tendon lime, pounded lime or colored lime.

[0051] Among them, the grass tendon ash is prepared by quicklime, dry rice straw and hemp silk in a weight ratio of 10-30:3-10:0.3-2.

[0052] The preparation method of grass tendon ash includes the following steps: first, mixing quicklime and rice straw evenly, then adding hemp silk and stirring thoroughly, and then sealing the mixture for soaking and fermentation. The fermentation time is 3-5 days to ensure that the lime and rice straw fully absorb water and soften. During this period, the mixture should be turned over every 8 hours to promote uniform fermentation and prevent local overheating. After the fermentation is completed, the mixture is dried for about 2-3 days until it is completely dry. Finally, fine grass tendon ash is obtained by grinding or crushing.

[0053] The straw paper tendon ash (straw tendon ash) is prepared by traditional process, which is made of quicklime, straw tendons and water in a certain proportion. In the embodiment of the present invention, fiber components such as rice straw, silk and hemp are introduced into the straw paper tendon ash, and the fiber components are combined with fermentation process to improve the toughness and crack resistance of the material.

[0054] Preferably, the temperature of the sealed fermentation of the straw ash or paper ash is 20-30° C. and the humidity is 60-80%.

[0055] Preferably, the quicklime in the grass ash is calcium quicklime of superior grade or above, the content of CaO in the calcium quicklime is above 85%, and the fineness is above 60 mesh.

[0056] Paper tendon ash is made from diluted ash paste, water, glutinous rice paste, and jade button paper, and is prepared in the ratio of 40-60:5-15:3-10:0.5-2.

[0057] The preparation method of the paper tendon ash comprises the following steps: firstly, lime paste, water, glutinous rice paste and jade button paper are mixed and stirred evenly, and then sealed and soaked for fermentation, and the fermentation time is 2-4 days to ensure that the raw materials fully absorb water and soften, and the mixture should be turned over every 8 hours during the fermentation to promote uniform fermentation and prevent local overheating. After the fermentation is completed, the mixture is dried, and the drying time is about 1-2 days until it is completely dry. Finally, fine paper tendon ash is obtained by grinding or crushing.

[0058] The traditional paper ash is made by first adding water to pure natural quicklime to make lime milk, then adding grass tendons in a certain proportion to make it into a slurry, and then flowing it into an ash storage tank to cool and solidify. In the embodiment of the present invention, jade button paper, glutinous rice flour, water and other ingredients are added to the paper ash, and the mixture is fully fermented and mixed, so that the material has good crack resistance.

[0059] Preferably, the temperature of the sealed fermentation of the straw ash or paper ash is 20-30° C. and the humidity is 60-80%.

[0060] Preferably, the glutinous rice slurry in the paper tendon ash is prepared from water and glutinous rice flour in a weight ratio of 1:2 to 1:3.

[0061] Preferably, the mass ratio of calcium oxide to water in the lime paste in the paper tendon ash is between 1:3 and 1:4.

[0062] The pounding ash is prepared by selecting prepared grass tendon ash and paper tendon ash, quicklime, brown sugar, glutinous rice flour and lime oil, and preparing them according to the weight ratio of 30-50:20-30:1-3:1-3:0.5-2:0.5-2.

[0063] The preparation method of pounded ash comprises the steps of: evenly mixing grass tendon ash, paper tendon ash, 1-3 parts by weight of quicklime, brown sugar, glutinous rice flour and lime oil, and repeatedly beating the mixture with a pestle for 30-60 minutes until the mixture becomes smooth and sticky.

[0064] Preferably, the lime oil in the pounded lime is prepared by mixing tung oil and slaked lime in a ratio of 1:3; the quicklime is calcium quicklime of superior grade or above, the content of CaO in the calcium quicklime is above 90%, and the fineness is above 60 mesh.

[0065] In traditional processes, the ash plastic materials usually only have grass root ash, paper tendon ash and color ash. In the embodiment of the present invention, the grass tendon ash and paper tendon ash are mixed, and then repeatedly pounded with brown sugar, quicklime, glutinous rice flour and lime oil, so that the material has better adhesion, and its toughness and crack resistance are improved. It can be directly used for ash coating and blank making of ash plastic products, and can be directly colored after the blank making is completed, without the need to first apply the grass tendon ash as the base, then shape the paper tendon ash, and then spread the color ash.

[0066] The color ash can be prepared by mixing the prepared mortar and pigment.

[0067] The method for preparing the color ash comprises the steps of: mixing the pounded ash prepared by the above preparation method with the pigment for 10-20 minutes to ensure that the pounded ash and the pigment are fully integrated. After the mixing is completed, the color ash needs to be left to stand for 12-24 hours to ensure that the pigment is fully penetrated.

[0068] Traditional colored ash is a mixture of paper tendon ash and pigment. In the scheme of the present invention, straw tendon ash and paper tendon ash are mixed, and then brown sugar, quicklime, glutinous rice flour, and lime oil are added to form pounded ash, which is then mixed with pigment to form colored ash. This can improve the color fastness of the colored ash, and make it resistant to cracking, aging, and fading.

[0069] The above-mentioned Lingnan gray plastic materials can be used to make gray plastic products.

[0070] Preferably, since the toughness and crack resistance of the material are improved, the mortar can be directly coated and molded in one step. Specifically, the manufacturing process may include the following steps:

[0071] Conception and design of patterns: Based on the architectural space and decoration requirements, combined with the pattern's theme, layout, color matching and cultural connotations, conceive and design a suitable gray sculpture pattern.

[0072] Measurement and design: According to the design pattern, the building parts are accurately measured, and the design pattern is appropriately adjusted and optimized according to the measurement results. Ensure that the plaster plastic can fit the installation position.

[0073] Sketching: According to the design pattern and measurement results, sketch the plastering sketch at the construction site to provide guidance for the subsequent frame making and plastering work.

[0074] Tie-bonded frame: According to the traditional craftsmanship and based on the sketch, steel nails can be driven into the corresponding parts of the building, and copper wire can be used to accurately and firmly bond the frame according to the sketch.

[0075] Lime wrapping: you can directly use pounded ash to wrap layer by layer on the modeling frame until the initial ash sculpture is completed; you can also use traditional production technology to first wrap grass root ash layer by layer on the modeling frame to form a prototype, complete the grass tendon ash base, and then add paper tendon ash.

[0076] Coloring: After the gray plastic is stabilized, it is colored according to the design pattern and color configuration. The coloring process follows the principle of gradual change. After each layer of color is applied, it takes 4 hours to make the gray plastic rich and natural in color.

[0077] Outline the lines: After coloring is completed, use tools such as carving knives and outline pens to outline the contours and details of the gray sculpture to enhance the three-dimensionality and layering of the gray sculpture.

[0078] Sealing and maintenance: After the gray plastic is completed, it should not be exposed to water within 5 days and should also be avoided from exposure to the sun.

[0079] Preferably, the skeleton can also be made by 3D printing technology, and then fixedly connected to the corresponding building parts. The corresponding gray plastic product manufacturing process specifically includes the following steps:

[0080] Measurement and modeling: According to the design pattern, the building parts are accurately measured, and the design pattern is appropriately adjusted and optimized according to the measurement results, and then the gray modeling skeleton is three-dimensionally modeled using 3DSMAX technology;

[0081] Printing the modeling skeleton: Import the gray modeling skeleton 3D model into the 3D printer, select the aluminum alloy material to print layer by layer, and make the modeling skeleton;

[0082] Install the modeling frame: fix the printed modeling frame to the building;

[0083] Wrapping the ash: Wrap the pounded ash layer by layer on the modeling frame, with each layer not exceeding 3 cm in thickness and with a time interval of not less than 24 hours, until the ash sculpture embryo is completed;

[0084] Coloring: After the gray plastic embryo is stable, use the gray color to color it according to the design pattern. Wait 4 hours after each layer of color;

[0085] Outlining: After coloring is completed, use the gray to outline the gray sculpture contours and detail lines;

[0086] Sealing and maintenance: Waterproof and sun-proof within 5 days after the gray plastic is completed.

[0087] The following is further described in conjunction with specific embodiments:

[0088] Example 1

[0089] A Lingnan lime plastic material, which includes grass root lime, paper tendon lime, pounded lime and colored lime.

[0090] Grass tendon ash is prepared by mixing quicklime, dry rice stalks and hemp fibers in a weight ratio of 20:5:1.

[0091] The preparation method of grass tendon ash includes the following steps: first, mixing quicklime and rice straw evenly, then adding hemp silk and stirring thoroughly, and then sealing the mixture for soaking and fermentation. The fermentation time is 4 days to ensure that the lime and rice straw fully absorb water and soften. During this period, the mixture should be turned over every 8 hours to promote uniform fermentation and prevent local overheating. After the fermentation is completed, the mixture is dried for about 3 days until it is completely dry. Finally, fine grass tendon ash is obtained by grinding or crushing.

[0092] The temperature of the sealed fermentation is controlled at 20-30°C, and the humidity is 60-80%. The quicklime is high-grade calcium quicklime, the CaO content in the calcium quicklime is about 90%, and the fineness is 60-80 mesh.

[0093] The paper ash is made of lime paste, water, glutinous rice paste, and jade button paper, which are prepared in the ratio of 50:10:5:1.

[0094] The preparation method of paper tendon ash includes the following steps: firstly, lime paste, water, glutinous rice paste and jade button paper are mixed and stirred evenly, and then sealed and soaked for fermentation for 3 days to ensure that the raw materials fully absorb water and soften. During the fermentation, the mixture should be turned over every 8 hours to promote uniform fermentation and prevent local overheating. After the fermentation is completed, the mixture is dried for about 2 days until it is completely dry. Finally, fine paper tendon ash is obtained by grinding or crushing.

[0095] Among them, the glutinous rice paste is prepared by water and glutinous rice flour in a weight ratio of 1:2.5, and the mass ratio of calcium oxide to water in the lime paste is about 1:3.5.

[0096] For pounding ash, select the prepared grass tendon ash and paper tendon ash, quicklime, brown sugar, glutinous rice flour and lime oil and prepare them in a weight ratio of 40:25:2:2:1:1.

[0097] The preparation method of pounded ash comprises the steps of: evenly mixing grass tendon ash, paper tendon ash, quicklime, brown sugar, glutinous rice flour and lime oil, and repeatedly beating the mixture with a pounding rod for 50 minutes until the mixture becomes smooth and sticky.

[0098] The lime oil is prepared by mixing cooked tung oil and lime in a ratio of 1:3; the quicklime is calcium quicklime of superior grade or above, the content of CaO in the calcium quicklime is above 90%, and the fineness is above 60 mesh.

[0099] The color ash can be prepared by selecting the prepared pounded ash and pigment and stirring them. Specifically, the preparation method of the color ash comprises the steps of: mixing the pounded ash prepared by the above preparation method and various required pigments for 10-20 minutes to ensure that the pounded ash and the pigment are fully integrated. After the mixing is completed, the color ash needs to be left to stand for 12-24 hours to ensure that the pigment is fully penetrated.

[0100] Example 2

[0101] A gray plastic product, reference Figure 1 , its manufacturing process may include the following steps:

[0102] S1-S4 prepares ash plastic materials. Specifically, the method of Example 1 can be referred to prepare grass root ash, paper tendon ash, pounded ash, and colored ash as needed.

[0103] S5 Conception and design of patterns: Based on the architectural space and decoration requirements, combined with the pattern's theme, layout, color matching and cultural connotations, conceive and design a suitable gray sculpture pattern.

[0104] S6 Measurement and Design: According to the design pattern, the building parts are accurately measured, and the design pattern is appropriately adjusted and optimized according to the measurement results. Ensure that the plaster plastic can fit the installation position.

[0105] S7 Sketching: Based on the design pattern and measurement results, sketch the plastering sketch at the construction site to provide guidance for the subsequent skeleton construction and plastering work.

[0106] S8: Make the frame: According to the sketch, drive steel nails into the corresponding parts of the building, and use copper wire to make the frame accurately and firmly according to the sketch.

[0107] S9: Wrap the prepared ash layer by layer on the modeling frame, carefully control the thickness of each layer to not exceed 3cm and the time interval to be no less than 24h, so that the ash material can be firmly wrapped until the ash sculpture embryo is completed.

[0108] S10 Coloring: After the gray plastic embryo is stable, use the prepared gray to color it according to the design pattern. The coloring process must follow the gradient principle. Wait 4 hours after each layer of color.

[0109] S11 Outlining: After coloring is completed, use tools such as carving knives and outline pens to outline the contours and details of the gray sculpture to enhance the three-dimensional and layered feel of the gray sculpture.

[0110] S12 Sealing and maintenance: After the completion of the plaster plastic, it should not be exposed to water within 5 days. When it rains, a cover should be made on the surface of the plaster plastic to prevent swelling. When the sunlight is strong, a layer of shade cover should be built on the plaster plastic to prevent ultraviolet radiation and cracks caused by exposure to the sun. The selected cover material is generally colorless, transparent, and matte material.

[0111] Example 3

[0112] A gray plastic product, reference Figure 2 , its manufacturing process may include the following steps:

[0113] S1-S4 prepares ash plastic materials. Specifically, the method of Example 1 can be referred to prepare grass root ash, paper tendon ash, pounded ash, and colored ash as needed.

[0114] S5 Conception and design of patterns: Based on the architectural space and decoration requirements, combined with the pattern's theme, layout, color matching and cultural connotations, conceive and design a suitable gray sculpture pattern.

[0115] S6 Measurement and Modeling: According to the design pattern, the building parts are accurately measured, and the design pattern is appropriately adjusted and optimized according to the measurement results to ensure that the plaster sculpture can fit the installation position, and the plaster sculpture modeling skeleton is three-dimensionally modeled using 3DSMAX technology.

[0116] At the same time, ABAQUS finite element analysis software can be used to perform mechanical analysis on the three-dimensional model of the modeling skeleton to ensure that it has sufficient bearing capacity and stability after printing.

[0117] S7 print modeling skeleton: In view of the light weight and high strength requirements of gray plastic, a low-density aluminum alloy material is selected. The specific mass percentage of each metal element is: 90% aluminum, 5% magnesium, 3% silicon, 1% copper and 1% zinc. The aluminum alloy material has good light weight and welding properties, with a density of about 2.7g / cm3, which is much lower than traditional steel and is easy to install and fix.

[0118] The three-dimensional model is imported into the 3D printer, and the above-mentioned low-density aluminum alloy material is used to print layer by layer to produce the modeling skeleton: the printing speed is adjusted to a stacking height of no more than 5mm per minute to ensure that the aluminum alloy material can be smoothly stacked and reduce thermal stress; the printing temperature is controlled between 400-450℃ to ensure that the aluminum alloy material maintains good fluidity and bonding during the printing process; the layer thickness is set to 0.2mm to improve printing accuracy and reduce printing time; the filling density is optimized to 90% to ensure that the printed skeleton has sufficient strength and stability. After the printing process is optimized, the tensile strength of the modeling skeleton reaches 360MPa, the yield strength reaches 280MPa, and the elongation reaches 9%, which can withstand various forces and deformations in the gray plastic production process.

[0119] S8 installs the modeling skeleton: transports the printed and processed modeling skeleton to the construction site and fixes it to the corresponding building part.

[0120] Specifically, refer to Figure 3-4 The 3D printed gray modeling frame 10 can be transported to the construction site first, and the connecting angle steel 30 can be implanted in the corresponding building part 40. The position and quantity of the connecting angle steel 30 should be reasonably arranged according to the design drawings and the installation requirements of the 3D printed gray modeling frame 10.

[0121] Correspondingly, the connecting steel sheet 20 is welded on the 3D printed gray modeling skeleton 10, and then the connecting steel sheet bolt holes 21 are aligned with the connecting angle steel bolt holes 31, and the 3D printed gray modeling skeleton 10 is connected and fixed with the implanted connecting angle steel 30 using bolts, and ensure that its verticality, horizontality and stability meet the design requirements.

[0122] Further, refer to Figure 5-6 , and the supporting structure can also be implanted in the corresponding building parts. The supporting structure can penetrate into the modeling frame and be welded and connected to the modeling frame to better support and fix the modeling frame.

[0123] The installation of the support structure can be done by first implanting the steel bars 50 in the corresponding building parts 40. Then, the steel bars 51 are welded to the fixed steel bars 50. The steel bars 51 should extend to both ends of the 3D printed gray modeling frame 10 so as to be welded and fixed to the 3D printed gray modeling frame 10. Finally, the steel bars 52 should be welded to the steel bars 50 to form several stable triangular structures, thereby building the entire support structure.

[0124] S9: Wrap the prepared ash layer by layer on the modeling frame, carefully control the thickness of each layer to not exceed 3cm and the time interval to be no less than 24h, so that the ash material can be firmly wrapped until the ash sculpture embryo is completed.

[0125] S10 Coloring: After the gray plastic embryo is stable, use the prepared gray to color it according to the design pattern. The coloring process must follow the gradient principle. Wait 4 hours after each layer of color.

[0126] S11 Outlining: After coloring is completed, use tools such as carving knives and outline pens to outline the contours and details of the gray sculpture to enhance the three-dimensional and layered feel of the gray sculpture.

[0127] S12 Sealing and maintenance: After the completion of the plaster plastic, it should not be exposed to water within 5 days. When it rains, a cover should be made on the surface of the plaster plastic to prevent swelling. When the sunlight is strong, a layer of shade cover should be built on the plaster plastic to prevent ultraviolet radiation and cracks caused by exposure to the sun. The selected cover material is generally colorless, transparent, and matte material.

[0128] Comparative Example 1

[0129] A ash plastic material, including at least one of grass root ash, paper tendon ash, pounded ash and colored ash.

[0130] Grass tendon ash is made from quicklime and hemp in a weight ratio of 20:1.

[0131] The preparation method of grass tendon ash includes the following steps: first, mixing quicklime and rice straw evenly, then sealing the mixture and soaking and fermenting it for 4 days to ensure that the lime and rice straw fully absorb water and soften, and turning the mixture every 8 hours to promote uniform fermentation and prevent local overheating. After fermentation, the mixture is air-dried for about 3 days until it is completely dry. Finally, fine grass tendon ash is obtained by grinding or crushing.

[0132] The temperature of the sealed fermentation is controlled at 20-30°C, and the humidity is 60-80%. The quicklime is high-grade calcium quicklime, the CaO content in the calcium quicklime is about 90%, and the fineness is 60-80 mesh.

[0133] Lime paste, water and glutinous rice slurry are selected for paper tendon ash and prepared in a ratio of 50:10:5. The preparation method of paper tendon ash includes the following steps: first, the lime paste, water and glutinous rice slurry are mixed and stirred evenly, and then sealed and soaked for fermentation. The fermentation time is 3 days to ensure that the raw materials fully absorb water and soften. During this period, the mixture should be turned over every 8 hours to promote uniform fermentation and prevent local overheating. After the fermentation is completed, the mixture is dried for about 2 days until it is completely dry. Finally, fine paper tendon ash is obtained by grinding or crushing.

[0134] Among them, the ratio of lime paste and glutinous rice paste is the same as that in Example 1.

[0135] The pounded ash is prepared by selecting the above-mentioned grass tendon ash and paper tendon ash, quicklime, brown sugar, glutinous rice flour, and lime oil, and preparing them in a weight ratio of 40:25:2:2:1:1.

[0136] The preparation method of pounded ash comprises the steps of: evenly mixing grass tendon ash, paper tendon ash, quicklime, brown sugar, glutinous rice flour and lime oil, and repeatedly beating the mixture with a pounding rod for 50 minutes until the mixture becomes smooth and sticky.

[0137] Lime oil and quicklime are the same as in Example 1.

[0138] The color ash can be prepared by selecting the prepared pounded ash and pigment and stirring them. Specifically, the preparation method of the color ash comprises the steps of: mixing the pounded ash prepared by the above preparation method and various required pigments for 10-20 minutes to ensure that the pounded ash and the pigment are fully integrated. After the mixing is completed, the color ash needs to be left to stand for 12-24 hours to ensure that the pigment is fully penetrated.

[0139] Comparative Example 2

[0140] A gray plastic product is produced by using the gray plastic material obtained in comparative example 1, and the production process is the same as that in example 2.

[0141] Table 1 is a comparison result of the performance test of the gray plastic products prepared by Example 2 of the present invention and Comparative Example 2. It can be seen that the gray plastic products prepared by the gray plastic materials of the embodiment of the present invention have significantly improved crack resistance and toughness.

[0142] Table 1 Comparison of properties of gray plastic products of Example 2 of the present invention and Comparative Example 2

[0143]

[0144] Comparative Example 3

[0145] A gray plastic product is made by using the gray plastic material obtained in Comparative Example 1, and the production process is as follows:

[0146] Making gray plastic material: making gray plastic material by the method of comparative example 1;

[0147] Conception and design of patterns: Based on the architectural space and decoration requirements, combined with the pattern's theme, layout, color matching and cultural connotations, conceive and design a suitable gray sculpture pattern.

[0148] Measurement and design: According to the design pattern, the building parts are accurately measured, and the design pattern is appropriately adjusted and optimized according to the measurement results. Ensure that the plaster plastic can fit the installation position.

[0149] Sketching: According to the design pattern and measurement results, sketch the plastering sketch at the construction site to provide guidance for the subsequent frame making and plastering work.

[0150] Make the frame: According to the sketch, hammer steel nails into the corresponding building parts, and use copper wire to make the frame accurately and firmly according to the sketch.

[0151] Wrapping ash: Wrap the prepared grass root ash layer by layer on the modeling skeleton, carefully controlling the thickness of each layer to not exceed 3cm and the time interval to be no less than 24h, so that the ash material can be firmly wrapped until the ash modeling prototype is completed and the grass reinforcement ash base is completed. One day after the grass reinforcement ash base is completed, spread the paper reinforcement ash to ensure that the paper reinforcement ash can be pressed tightly on the grass root ash. During the spreading process, pay attention to the thickness of each time not exceeding 2 cm.

[0152] Coloring: After the gray plastic embryo is stable, color it according to the design pattern using the gray prepared in Example 1. The coloring process must follow the principle of gradual change, and wait 4 hours after each layer of color is applied.

[0153] Outline the lines: After coloring is completed, use tools such as carving knives and outline pens to outline the contours and details of the gray sculpture to enhance the three-dimensionality and layering of the gray sculpture.

[0154] Sealing and maintenance: After the completion of the plaster plastic, it cannot be exposed to water within 5 days. When it rains, a cover should be made on the surface of the plaster plastic to prevent swelling. When the sunlight is strong, a layer of shade cover should be built on the plaster plastic to prevent ultraviolet radiation and cracks caused by exposure to the sun. The selected cover material is generally colorless, transparent, and matte material.

[0155] The product manufacturing process in Example 3 of the present invention is compared with the product manufacturing process in Comparative Example 3, and the construction effect is shown in Table 2. It can be seen that the manufacturing process in Example 3 of the present invention can greatly reduce the construction time and improve the yield rate by combining 3D printing and the improvement of the plastering process brought about by material improvement.

[0156] Table 2 is a comparison of the construction effects of the gray plastic production process of Examples 2-3 of the present invention and Comparative Example 3

[0157]

[0158] In summary, compared with the prior art, the beneficial effects of the present invention are mainly reflected in the innovation of gray plastic materials and gray plastic product manufacturing processes. By adding materials such as dry straw and jade button paper and improving the material manufacturing process, the crack resistance and toughness of the gray plastic are significantly improved, thereby extending its service life; at the same time, the improved gray plastic material reduces the construction difficulty of the gray wrapping process, and further combined with 3D printing to produce gray plastic skeletons, it can greatly improve construction efficiency and improve the yield rate, which is conducive to the inheritance and development of gray plastic technology. In summary, the present invention improves the durability, aesthetics and ease of construction of gray plastic as a whole.

[0159] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0160] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing Lingnan gray plastic material, characterized in that: The ash plastic material includes at least one of grass root ash, paper tendon ash, pounded ash, or colored ash. The preparation method of the grass tendon ash comprises the following steps: firstly, 10-30 parts by weight of quicklime and 3-10 parts by weight of rice straw are uniformly mixed, then 0.3-2 parts by weight of hemp silk are added and fully stirred, then the mixture is sealed, soaked and fermented, the fermentation time is 3-5 days, the mixture should be turned over every 8 hours during the fermentation period, after the fermentation is completed, the mixture is dried, and then ground or crushed to obtain the grass tendon ash; The preparation method of the paper tendon ash comprises the following steps: firstly, 40-60 parts by weight of lime paste, 5-15 parts by weight of water, 3-10 parts by weight of glutinous rice paste, and 0.5-2 parts by weight of jade button paper are mixed and stirred evenly, and then sealed, soaked and fermented for 2-4 days, and the mixture is turned over every 8 hours. After the fermentation is completed, the mixture is dried, and then ground or crushed to obtain the grass tendon ash; The preparation method of pounded ash comprises the following steps: evenly mixing 30-50 parts by weight of grass tendon ash prepared by the preparation method, 20-30 parts by weight of paper tendon ash prepared by the preparation method, 1-3 parts by weight of quicklime, 1-3 parts by weight of brown sugar, 0.5-2 parts by weight of glutinous rice flour, and 0.5-2 parts by weight of lime oil, and repeatedly beating the mixture with a pestle for 30-60 minutes until the mixture becomes smooth and sticky; The method for preparing the colored ash comprises the steps of: mixing the pounded ash and the pigment for 10-20 minutes and then standing for 12-24 hours.

2. The preparation method according to claim 1, characterized in that: The sealed fermentation temperature of the straw ash or paper ash is 20-30° C. and the humidity is 60-80%.

3. The preparation method according to claim 1, characterized in that: The quicklime in the grass ash is calcium quicklime of superior grade or above, the content of CaO in the calcium quicklime is above 85%, and the fineness is above 60 meshes.

4. The preparation method according to claim 1, characterized in that: In the glutinous rice slurry of the paper tendon ash, the weight ratio of water to glutinous rice flour is 1:2 to 1:

3.

5. The preparation method according to claim 1, characterized in that: The mass ratio of calcium oxide to water in the lime paste in the paper tendon ash is between 1:3 and 1:

4.

6. The preparation method according to claim 1, characterized in that: The lime oil in the pounded lime is prepared by mixing slaked lime and tung oil in a mass ratio of 3:1; The quicklime is calcium quicklime of superior grade or above, the content of CaO in the calcium quicklime is above 85%, and the fineness is above 60 meshes.

7. Lingnan gray plastic material prepared by the preparation method as described in any one of claims 1-6.

8. A gray plastic product, characterized in that: It is made from the gray plastic material as described in claim 7.

9. The process for producing a gray plastic product according to claim 8, characterized in that: The steps include: Conceive and design patterns; measurement and design; sketch; Tie up the modeling frame; Wrapping the ash: Wrap the pounded ash layer by layer on the modeling frame, with each layer not exceeding 3 cm in thickness and with a time interval of not less than 24 hours, until the ash sculpture embryo is completed; Coloring: After the gray plastic embryo is stable, use the gray color to color it according to the design pattern. Wait 4 hours after each layer of color; Outlining the lines: After coloring is completed, use the gray to outline the gray sculpture contours and detail lines; Sealing and maintenance: Waterproof and sun-proof within 5 days after the gray plastic is completed.

10. The process for producing a gray plastic product according to claim 8, characterized in that: The steps include: Conceive and design patterns; Measurement and modeling: According to the design pattern, the building parts are accurately measured, and the design pattern is adjusted and optimized according to the measurement results. Then, the gray modeling skeleton is 3D modeled using 3DSMAX technology; Printing the modeling skeleton: Import the gray modeling skeleton 3D model into the 3D printer, select the aluminum alloy material to print layer by layer, and make the modeling skeleton; Install the modeling frame: fix the printed modeling frame to the building; Wrapping the ash: Wrap the pounded ash layer by layer on the modeling frame, with each layer not exceeding 3 cm in thickness and with a time interval of not less than 24 hours, until the ash sculpture embryo is completed; Coloring: After the gray plastic embryo is stable, use the gray color to color it according to the design pattern. Wait 4 hours after each layer of color; Outlining the lines: After coloring is completed, use the gray to outline the gray sculpture contours and detail lines; Sealing and maintenance: Waterproof and sun-proof within 5 days after the gray plastic is completed.

Citation Information

Patent Citations

  • Method for preparing grey plaster used paper strip mixed lime mortar material by adopting celluloses

    CN104386934A

  • Outer wall clay sculpture construction method and mortar adopted in same

    CN104712114A

  • Lime model environment-friendly building material and preparation method and application thereof

    CN106045438A

  • Manufacturing process of high-hardness stucco sculpture product

    CN113880499A

  • High-performance plastering construction method suitable for traditional building roof ridge wrapping and wall surface

    CN114293721A

Cited By

  • Mould forming Lingnan grey sculpture embossment construction method based on AI generative design

    CN119636290A