Toughened mullite ceramic and preparation method thereof

By adding mullite fibers and alumina particles to the ceramic material and combining with the kiln process, the problem of insufficient fracture toughness of ceramic materials is solved, and the mechanical properties and toughness of ceramics are significantly improved.

CN118908694APending Publication Date: 2024-11-08XINHUA COUNTY SHUNDA ELECTRONIC CERAMICS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411180390.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The fracture toughness and relative strength of existing ceramic materials are low, and cracks and fractures are prone to occur on the surface of the ceramic, affecting the quality of the ceramic.

Method used

Ceramic blanks are made of kaolinite, mica, mullite fiber, alumina particles, concave and concave rock stone and graphene, and are made into pottery through crushing, screening, ball milling, mixing, and firing processes, adding Molai Stone fibers and alumina particles to improve the mechanical properties of ceramics.

Benefits of technology

The fracture toughness and relative strength of the composite material are significantly enhanced, and crack propagation is prevented through the bridge of mullite fibers and the plastic deformation effect of alumina particles, thereby improving the mechanical properties of the ceramics.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses toughened mullite ceramic and a preparation method thereof.The toughened mullite ceramic is prepared from, by weight, 80-120 parts of ceramic blank, 20-40 parts of kaolinite, 8-20 parts of hydromuscovite, 4-8 parts of mullite fiber, 6-12 parts of aluminum oxide particles, 14-24 parts of attapulgite and 6-12 parts of graphene, and relates to the technical field of ceramic materials. The mechanical property of the ceramic is improved by adopting a method of adding mullite, the mullite is uniformly added into the ceramic material, and the mullite is used as a toughening phase of a matrix, so that the fracture toughness and the relative strength of the composite material are remarkably enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic materials, and in particular to a toughened mullite ceramic and a preparation method thereof. Background Art

[0002] Pottery is a utensil made of clay or pottery that is kneaded and then fired. Pottery has a long history, and simple and crude pottery was first seen in the Neolithic Age. Pottery was used as a daily necessity in ancient times, and is now generally collected as a handicraft.

[0003] There are generally four methods for ceramic toughening: dispersion toughening, phase change toughening, fiber and whisker toughening, and the recently developed carbon nanotube toughening. Among them, the effect of dispersion toughening is very limited; although the phase change toughening of zirconia ceramics can increase the fracture toughness of the material by 2 to 3 times, the effect of phase change toughening drops sharply with the increase of temperature; carbon nanotubes are easily damaged in the process of mass production, dispersion and subsequent sintering, and the synthesis process is complex and expensive, so their application is limited. The obvious toughening effect and good high temperature performance make the use of fiber and whisker toughening the first choice and research focus of ceramic toughening.

[0004] The stoichiometric formula of mullite is 3Al2O3·2SiO2. It has stable chemical properties and is insoluble in hydrofluoric acid. It has uniform thermal expansion coefficient, good thermal shock resistance, high load softening point, high refractoriness, low creep, high hardness and good chemical corrosion resistance, which makes it important in high-temperature refractory materials, electronic packaging materials, optical materials, dielectric and high-temperature protective coatings. Since natural mullite with economic value is very rare in the earth's crust, it needs to be synthesized from natural raw materials or industrial raw materials, including high-alumina bauxite, sillimanite minerals, pyrope, kaolin, clay, wax stone and silica, etc. Industrial raw materials include industrial alumina, α-Al2O3 powder, aluminum hydroxide, etc. Researchers are also studying the use of sol-gel and coprecipitation methods supplemented by high-temperature calcination to obtain mullite powder in advance.

[0005] Patent Publication No.: CN104529421A, mullite precursor powder is prepared by sol-gel method, and then sintered in spark plasma sintering furnace, the sintering temperature is 1400℃, pressurization starts when the temperature reaches 1150℃, the pressure is 80MPa, and the heating rate is greater than 90℃ / min; in the later stage of sintering, the heating rate starts to be reduced at an appropriate temperature point to prepare mullite ceramics with fine grains.

[0006] Existing ceramic composite materials are deficient in fracture toughness and relative strength, the mechanical properties of ceramics are relatively poor, and cracks and fractures are easily present on the ceramic surface, which affects the quality of the ceramics. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides a toughened mullite ceramic and a preparation method thereof, which is composed of the following parts by weight: 80-120 parts by weight of ceramic blank, 20-40 parts by weight of kaolinite, 8-20 parts by weight of hydromuscovite, 4-8 parts by weight of mullite fiber, 6-12 parts by weight of alumina particles, 14-24 parts by weight of attapulgite and 6-12 parts by weight of graphene.

[0008] Preferably, the ceramic blank is composed of the following parts by weight: 20-60 parts by weight of lithium mica tailings, 20-40 parts by weight of wollastonite tailings, 16-36 parts by weight of clay, 5-20 parts by weight of potassium feldspar, 5-20 parts by weight of sodium feldspar and 4-16 parts by weight of quartz.

[0009] A method for preparing toughened mullite ceramics comprises the following steps: Step 1: crushing kaolinite, quartz, hydromucovite, attapulgite and graphene, sieving the crushed kaolinite, quartz, hydromucovite, attapulgite and graphene, and reserving the sieved powder for later use; Step 2: mixing the sieved powder with mullite fibers and alumina particles, and ball milling the mixture using a ball mill, and setting the milled powder aside; Step 3: mixing the ball-milled powder with the ceramic blank, and adding an appropriate amount of tap water to the mixture to obtain a mixture; Step 4: The mixture is made into pottery through conventional embryo pulling, embryo drying and kiln firing processes.

[0010] Preferably, the method for preparing the ceramic blank comprises the following steps: Step 1: Prepare materials by weight, including lithium mica tailings, wollastonite tailings, clay, potassium feldspar, sodium feldspar, and quartz; Step 2: crush and screen the prepared mica tailings, wollastonite tailings, clay, potassium feldspar, sodium feldspar and quartz for later use; Step 3: Mix the mica tailings, wollastonite tailings, clay, potassium feldspar, sodium feldspar and quartz screened in step 2 to obtain a mixed blank; Step 4: wet ball milling the mixed blank to obtain blank slurry; Step 5: removing iron from the green body slurry and spray drying it to obtain a ceramic green body.

[0011] Preferably, the method for preparing the mullite fiber comprises the following steps: Step 1: Add aluminum chloride solution and aluminum powder in proportion to a heating and reflux reactor, heat at 95-110°C for 1.5-3h, and after the reaction is complete, filter to obtain a pale transparent polyaluminum chloride mother liquor; Step 2: adding a blend of tetraethoxysilane and anhydrous ethanol to a mixed solution of nitric acid and acetic acid, stirring for 0.8 h, the tetraethoxysilane is hydrolyzed to obtain a silicic acid solution; Step 3: adding the obtained silicic acid solution to the polyaluminium chloride mother liquor, adding acetic acid as a stabilizer and a spinning aid or other oxide second phase precursor sol, vacuum concentrating at 70-80° C. to obtain a mullite fiber precursor sol having a viscosity of 15-35 Pa·s; Step 4: centrifugal spinning is performed using a homemade centrifugal spinning machine to finally obtain gel fibers with uniform diameter; Step 5: Dry the obtained gel fiber at 50-70°C for 24 hours, and heat treat at 950-1500°C for 2 hours to obtain the desired mullite fiber.

[0012] Preferably, the centrifugal spinning process in step four is as follows: the precursor sol is centrifuged at high speed from a small hole with a pore size of 0.45 mm under the action of centrifugal force, and then secondary pulled by a hot air flow of 50-70°C, dried and solidified, finally obtaining precursor long fibers with uniform diameter and good toughness.

[0013] Preferably, the molar ratio of the anhydrous aluminum chloride to the aluminum powder is 1.7:2.1, preferably 1.8:2.0.

[0014] Preferably, the oxide second phase is one of MgO, B2O3, Y2O3, and ZrO2, and the precursor sol is magnesium acetate solution, boric acid solution, yttrium acetate solution, and zirconium acetate solution, respectively.

[0015] Preferably, the volume ratio of tetraethoxysilane, anhydrous ethanol, concentrated nitric acid, acetic acid and water is 10:5:1:1:15.

[0016] The present invention provides a toughened mullite ceramic and a preparation method thereof. It has the following beneficial effects: 1. The present invention adopts the method of adding mullite to improve the mechanical properties of ceramics. Mullite is evenly added to the ceramic material, wherein the mullite serves as a toughening phase of the matrix, which significantly enhances the fracture toughness and relative strength of the composite material.

[0017] 2. The present invention adds alumina particles to the traditional clay formula for toughening. Through the dispersion of alumina particles or the movement of particles, a certain plastic deformation is produced, creep is caused by sliding along the crystal interface, crack tip shielding is formed, micro cracks or crack bridges are formed around the main crack, and the residual thermal stress caused by the mismatch between the phase thermal expansion coefficient and elastic modulus of alumina and the matrix such as kaolinite and quartz interacts with the stress at the tip of the diffusion crack, so that the crack produces deflection, bifurcation, bridging or pinning effects, thereby preventing crack propagation and improving fracture toughness.

[0018] 3. The present invention adds mullite fiber, which has multiple toughening and strengthening mechanisms such as bridging, crack deflection (or bifurcation) and fiber pullout. When bridging occurs, the mullite fiber pulls the two crack surfaces like a bridge to prevent the crack from further expanding. The bonding surface between the mullite fiber and the ceramic matrix is ​​a weak bonding surface. When the fracture strength of the mullite exceeds the expansion stress of the crack, the crack deviates from the original direction of advance and expands along the bonding surface between the mullite fiber and the matrix, causing interface dissociation. When the expansion stress is greater than the fracture strength of the mullite fiber, the crack passes through the mullite fiber. The crack expansion path is serrated, has a larger surface area and surface energy than a plane crack, can absorb more energy, and has a toughening effect.

[0019] 4. The present invention utilizes lithium mica tailings with low sintering temperature to prepare ceramic green bodies. Adding a large proportion of lithium mica tailings into the ceramic green bodies can effectively reduce the proportion of other raw materials added, thereby achieving the purpose of consuming tailings and waste slag, and reducing the firing temperature and production cost of the ceramic green bodies, turning waste into treasure and realizing green and low-carbon production. DETAILED DESCRIPTION

[0020] The following specific embodiments further describe the present invention in detail. The embodiments of the present invention are provided for the purpose of illustration and description, and are not intended to be exhaustive or to limit the present invention to the disclosed forms. Many modifications and variations will be apparent to those of ordinary skill in the art. The embodiments are selected and described to better illustrate the principles and practical applications of the present invention, and to enable those of ordinary skill in the art to understand the present invention and thereby design various embodiments with various modifications suitable for specific uses.

[0021] Example 1, a toughened mullite ceramic, composed of the following parts by weight: 80 parts by weight of ceramic green body, 20 parts by weight of kaolinite, 8 parts by weight of hydromuscovite, 4 parts by weight of mullite fiber, 6 parts by weight of alumina particles, 14 parts by weight of attapulgite and 6 parts by weight of graphene.

[0022] The ceramic blank is composed of the following parts by weight: 20 parts by weight of lithium mica tailings, 20 parts by weight of wollastonite tailings, 16 parts by weight of clay, 5 parts by weight of potassium feldspar, 5 parts by weight of sodium feldspar and 4 parts by weight of quartz.

[0023] A method for preparing toughened mullite ceramics comprises the following steps: Step 1: crushing kaolinite, quartz, hydromucovite, attapulgite and graphene, sieving the crushed kaolinite, quartz, hydromucovite, attapulgite and graphene, and reserving the sieved powder for later use; Step 2: Mix the sieved powder with mullite fiber and alumina particles, and use a ball mill to perform ball milling. The ball milled powder is set aside; Step 3: Mix the ball-milled powder with the ceramic blank, and add an appropriate amount of tap water to the mixture to obtain a mixture; Step 4: The mixture is made into pottery through conventional embryo pulling, embryo drying and kiln firing processes.

[0024] The method for preparing the ceramic blank comprises the following steps: Step 1: Prepare materials by weight, including lithium mica tailings, wollastonite tailings, clay, potassium feldspar, sodium feldspar, and quartz; Step 2: crush and screen the prepared mica tailings, wollastonite tailings, clay, potassium feldspar, sodium feldspar and quartz for later use; Step 3: Mix the mica tailings, wollastonite tailings, clay, potassium feldspar, sodium feldspar and quartz screened in step 2 to obtain a mixed blank; Step 4: wet ball milling the mixed blank to obtain blank slurry; Step 5: Remove iron from the green body slurry and spray dry it to obtain a ceramic green body.

[0025] The preparation method of mullite fiber comprises the following steps: Step 1: Add aluminum chloride solution and aluminum powder in proportion to a heating and reflux reactor, heat at 95-110°C for 1.5-3h, and after the reaction is complete, filter to obtain a pale transparent polyaluminum chloride mother liquor; Step 2: adding a blend of tetraethoxysilane and anhydrous ethanol to a mixed solution of nitric acid and acetic acid, stirring for 0.8 h, the tetraethoxysilane is hydrolyzed to obtain a silicic acid solution; Step 3: adding the obtained silicic acid solution to the polyaluminium chloride mother liquor, adding acetic acid as a stabilizer and a spinning aid or other oxide second phase precursor sol, vacuum concentrating at 70-80° C. to obtain a mullite fiber precursor sol having a viscosity of 15-35 Pa·s; Step 4: centrifugal spinning is performed using a homemade centrifugal spinning machine to finally obtain gel fibers with uniform diameter; Step 5: Dry the obtained gel fiber at 50-70°C for 24 hours, and heat treat at 950-1500°C for 2 hours to obtain the desired mullite fiber.

[0026] The centrifugal spinning process in step four is as follows: under the action of centrifugal force, the precursor sol is centrifugally thrown out at high speed from a small hole with an aperture of 0.45 mm, and then pulled for the second time by a hot air flow of 50-70°C, dried and solidified, and finally a precursor long fiber with uniform diameter and good toughness is obtained. The fiber length is 35-70cm and the diameter is 10-20um. Among them, the diameter of the spinning head is 50mm and the height is 40mm. There are 16 small holes with a diameter of 0.45mm evenly distributed around it. The speed of the centrifuge is 2500-3500r / min, the temperature in the fiber forming hood is 55-70°C, and the relative humidity is 22%-45%.

[0027] The second oxide phase is one of MgO, B2O3, Y2O3, and ZrO2, and the precursor sols are magnesium acetate solution, boric acid solution, yttrium acetate solution, and zirconium acetate solution, respectively.

[0028] The process of heat treatment of the gel fiber in step five is as follows: put the gel fiber into a heat treatment furnace, heat it from 100°C to 600°C at a rate of 1.5°C / min, and keep it warm for 1 hour, wherein water vapor is introduced at 200-500°C to remove the acidic volatile gas produced by fiber pyrolysis, so that the fiber surface is not corroded; then heat it to 700°C at a rate of 3°C / min, and keep it warm for 1 hour; finally, heat the fiber to above 1300°C at 5°C / min, and keep it warm for 2 hours to obtain the mullite fiber to be prepared.

[0029] Example 2, a toughened mullite ceramic, composed of the following parts by weight: 100 parts by weight of ceramic green body, 30 parts by weight of kaolinite, 14 parts by weight of hydromuscovite, 6 parts by weight of mullite fiber, 9 parts by weight of alumina particles, 19 parts by weight of attapulgite and 9 parts by weight of graphene.

[0030] The ceramic blank is composed of the following parts by weight: 40 parts by weight of lithium mica tailings, 30 parts by weight of wollastonite tailings, 26 parts by weight of clay, 12.5 parts by weight of potassium feldspar, 12.5 parts by weight of sodium feldspar and 10 parts by weight of quartz.

[0031] A method for preparing toughened mullite ceramics comprises the following steps: Step 1: crushing kaolinite, quartz, hydromucovite, attapulgite and graphene, sieving the crushed kaolinite, quartz, hydromucovite, attapulgite and graphene, and reserving the sieved powder for later use; Step 2: Mix the sieved powder with mullite fiber and alumina particles, and use a ball mill to perform ball milling. The ball milled powder is set aside; Step 3: Mix the ball-milled powder with the ceramic blank, and add an appropriate amount of tap water to the mixture to obtain a mixture; Step 4: The mixture is made into pottery through conventional embryo pulling, embryo drying and kiln firing processes.

[0032] The method for preparing the ceramic blank comprises the following steps: Step 1: Prepare materials by weight, including lithium mica tailings, wollastonite tailings, clay, potassium feldspar, sodium feldspar, and quartz; Step 2: crush and screen the prepared mica tailings, wollastonite tailings, clay, potassium feldspar, sodium feldspar and quartz for later use; Step 3: Mix the mica tailings, wollastonite tailings, clay, potassium feldspar, sodium feldspar and quartz screened in step 2 to obtain a mixed blank; Step 4: wet ball milling the mixed blank to obtain blank slurry; Step 5: Remove iron from the green body slurry and spray dry it to obtain a ceramic green body.

[0033] The preparation method of mullite fiber comprises the following steps: Step 1: Add aluminum chloride solution and aluminum powder in proportion to a heating and reflux reactor, heat at 95-110°C for 1.5-3h, and after the reaction is complete, filter to obtain a pale transparent polyaluminum chloride mother liquor; Step 2: adding a blend of tetraethoxysilane and anhydrous ethanol to a mixed solution of nitric acid and acetic acid, stirring for 0.8 h, the tetraethoxysilane is hydrolyzed to obtain a silicic acid solution; Step 3: adding the obtained silicic acid solution to the polyaluminium chloride mother liquor, adding acetic acid as a stabilizer and a spinning aid or other oxide second phase precursor sol, vacuum concentrating at 70-80° C. to obtain a mullite fiber precursor sol having a viscosity of 15-35 Pa·s; Step 4: centrifugal spinning is performed using a homemade centrifugal spinning machine to finally obtain gel fibers with uniform diameter; Step 5: Dry the obtained gel fiber at 50-70°C for 24 hours, and heat treat at 950-1500°C for 2 hours to obtain the desired mullite fiber.

[0034] The centrifugal spinning process in step four is as follows: under the action of centrifugal force, the precursor sol is centrifugally thrown out at high speed from a small hole with an aperture of 0.45 mm, and then pulled for the second time by a hot air flow of 50-70°C, dried and solidified, and finally a precursor long fiber with uniform diameter and good toughness is obtained. The fiber length is 35-70cm and the diameter is 10-20um. Among them, the diameter of the spinning head is 50mm and the height is 40mm. There are 16 small holes with a diameter of 0.45mm evenly distributed around it. The speed of the centrifuge is 2500-3500r / min, the temperature in the fiber forming hood is 55-70°C, and the relative humidity is 22%-45%.

[0035] The second oxide phase is one of MgO, B2O3, Y2O3, and ZrO2, and the precursor sols are magnesium acetate solution, boric acid solution, yttrium acetate solution, and zirconium acetate solution, respectively.

[0036] The process of heat treatment of the gel fiber in step five is as follows: put the gel fiber into a heat treatment furnace, heat it from 100°C to 600°C at a rate of 1.5°C / min, and keep it warm for 1 hour, wherein water vapor is introduced at 200-500°C to remove the acidic volatile gas produced by fiber pyrolysis, so that the fiber surface is not corroded; then heat it to 700°C at a rate of 3°C / min, and keep it warm for 1 hour; finally, heat the fiber to above 1300°C at 5°C / min, and keep it warm for 2 hours to obtain the mullite fiber to be prepared.

[0037] Example 3, a toughened mullite ceramic, composed of the following parts by weight: 80-120 parts by weight of ceramic green body, 20-40 parts by weight of kaolinite, 8-20 parts by weight of hydromuscovite, 4-8 parts by weight of mullite fiber, 6-12 parts by weight of alumina particles, 14-24 parts by weight of attapulgite and 6-12 parts by weight of graphene.

[0038] The ceramic blank is composed of the following parts by weight: 60 parts by weight of lithium mica tailings, 40 parts by weight of wollastonite tailings, 36 parts by weight of clay, 20 parts by weight of potassium feldspar, 20 parts by weight of sodium feldspar and 16 parts by weight of quartz.

[0039] A method for preparing toughened mullite ceramics comprises the following steps: Step 1: crushing kaolinite, quartz, hydromucovite, attapulgite and graphene, sieving the crushed kaolinite, quartz, hydromucovite, attapulgite and graphene, and reserving the sieved powder for later use; Step 2: Mix the sieved powder with mullite fiber and alumina particles, and use a ball mill to perform ball milling. The ball milled powder is set aside; Step 3: Mix the ball-milled powder with the ceramic blank, and add an appropriate amount of tap water to the mixture to obtain a mixture; Step 4: The mixture is made into pottery through conventional embryo pulling, embryo drying and kiln firing processes.

[0040] The method for preparing the ceramic blank comprises the following steps: Step 1: Prepare materials by weight, including lithium mica tailings, wollastonite tailings, clay, potassium feldspar, sodium feldspar, and quartz; Step 2: crush and screen the prepared mica tailings, wollastonite tailings, clay, potassium feldspar, sodium feldspar and quartz for later use; Step 3: Mix the mica tailings, wollastonite tailings, clay, potassium feldspar, sodium feldspar and quartz screened in step 2 to obtain a mixed blank; Step 4: wet ball milling the mixed blank to obtain blank slurry; Step 5: Remove iron from the green body slurry and spray dry it to obtain a ceramic green body.

[0041] The preparation method of mullite fiber comprises the following steps: Step 1: Add aluminum chloride solution and aluminum powder in proportion to a heating and reflux reactor, heat at 95-110°C for 1.5-3h, and after the reaction is complete, filter to obtain a pale transparent polyaluminum chloride mother liquor; Step 2: adding a blend of tetraethoxysilane and anhydrous ethanol to a mixed solution of nitric acid and acetic acid, stirring for 0.8 h, the tetraethoxysilane is hydrolyzed to obtain a silicic acid solution; Step 3: adding the obtained silicic acid solution to the polyaluminium chloride mother liquor, adding acetic acid as a stabilizer and a spinning aid or other oxide second phase precursor sol, vacuum concentrating at 70-80° C. to obtain a mullite fiber precursor sol having a viscosity of 15-35 Pa·s; Step 4: centrifugal spinning is performed using a homemade centrifugal spinning machine to finally obtain gel fibers with uniform diameter; Step 5: Dry the obtained gel fiber at 50-70°C for 24 hours, and heat treat at 950-1500°C for 2 hours to obtain the desired mullite fiber.

[0042] The centrifugal spinning process in step four is as follows: under the action of centrifugal force, the precursor sol is centrifugally thrown out at high speed from a small hole with an aperture of 0.45 mm, and then pulled for the second time by a hot air flow of 50-70°C, dried and solidified, and finally a precursor long fiber with uniform diameter and good toughness is obtained. The fiber length is 35-70cm and the diameter is 10-20um. Among them, the diameter of the spinning head is 50mm and the height is 40mm. There are 16 small holes with a diameter of 0.45mm evenly distributed around it. The speed of the centrifuge is 2500-3500r / min, the temperature in the fiber forming hood is 55-70°C, and the relative humidity is 22%-45%.

[0043] The second oxide phase is one of MgO, B2O3, Y2O3, and ZrO2, and the precursor sols are magnesium acetate solution, boric acid solution, yttrium acetate solution, and zirconium acetate solution, respectively.

[0044] The process of heat treatment of the gel fiber in step five is as follows: put the gel fiber into a heat treatment furnace, heat it from 100°C to 600°C at a rate of 1.5°C / min, and keep it warm for 1 hour, wherein water vapor is introduced at 200-500°C to remove the acidic volatile gas produced by fiber pyrolysis, so that the fiber surface is not corroded; then heat it to 700°C at a rate of 3°C / min, and keep it warm for 1 hour; finally, heat the fiber to above 1300°C at 5°C / min, and keep it warm for 2 hours to obtain the mullite fiber to be prepared.

[0045] Example 4, a toughened mullite ceramic, composed of the following parts by weight: 100 parts by weight of ceramic green body, 30 parts by weight of kaolinite, 14 parts by weight of hydromuscovite, 6 parts by weight of mullite fiber, 9 parts by weight of alumina particles, 19 parts by weight of attapulgite and 9 parts by weight of graphene.

[0046] The ceramic blank is composed of the following parts by weight: 40 parts by weight of lithium mica tailings, 30 parts by weight of wollastonite tailings, 26 parts by weight of clay, 12.5 parts by weight of potassium feldspar, 12.5 parts by weight of sodium feldspar and 10 parts by weight of quartz.

[0047] A method for preparing toughened mullite ceramics comprises the following steps: Step 1: crushing kaolinite, quartz, hydromucovite, attapulgite and graphene, sieving the crushed kaolinite, quartz, hydromucovite, attapulgite and graphene, and reserving the sieved powder for later use; Step 2: Mix the sieved powder with mullite fiber and alumina particles, and use a ball mill to perform ball milling. The ball milled powder is set aside; Step 3: Mix the ball-milled powder with the ceramic blank, and add an appropriate amount of tap water to the mixture to obtain a mixture; Step 4: The mixture is made into pottery through conventional embryo pulling, embryo drying and kiln firing processes.

[0048] The method for preparing the ceramic blank comprises the following steps: Step 1: Prepare materials by weight, including lithium mica tailings, wollastonite tailings, clay, potassium feldspar, sodium feldspar, and quartz; Step 2: crush and screen the prepared mica tailings, wollastonite tailings, clay, potassium feldspar, sodium feldspar and quartz for later use; Step 3: Mix the mica tailings, wollastonite tailings, clay, potassium feldspar, sodium feldspar and quartz screened in step 2 to obtain a mixed blank; Step 4: wet ball milling the mixed blank to obtain blank slurry; Step 5: Remove iron from the green body slurry and spray dry it to obtain a ceramic green body.

[0049] The preparation method of mullite fiber comprises the following steps: Step 1: Add aluminum chloride solution and aluminum powder in proportion to a heating and reflux reactor, heat at 95-110°C for 1.5-3h, and after the reaction is complete, filter to obtain a pale transparent polyaluminum chloride mother liquor; Step 2: adding a blend of tetraethoxysilane and anhydrous ethanol to a mixed solution of nitric acid and acetic acid, stirring for 0.8 h, the tetraethoxysilane is hydrolyzed to obtain a silicic acid solution; Step 3: adding the obtained silicic acid solution to the polyaluminium chloride mother liquor, adding acetic acid as a stabilizer and a spinning aid or other oxide second phase precursor sol, vacuum concentrating at 70-80° C. to obtain a mullite fiber precursor sol having a viscosity of 15-35 Pa·s; Step 4: centrifugal spinning is performed using a homemade centrifugal spinning machine to finally obtain gel fibers with uniform diameter; Step 5: Dry the obtained gel fiber at 50-70°C for 24 hours, and heat treat at 950-1500°C for 2 hours to obtain the desired mullite fiber.

[0050] The centrifugal spinning process in step four is as follows: under the action of centrifugal force, the precursor sol is centrifugally thrown out at high speed from a small hole with an aperture of 0.45 mm, and then pulled for the second time by a hot air flow of 50-70°C, dried and solidified, and finally a precursor long fiber with uniform diameter and good toughness is obtained. The fiber length is 35-70cm and the diameter is 10-20um. Among them, the diameter of the spinning head is 50mm and the height is 40mm. There are 16 small holes with a diameter of 0.45mm evenly distributed around it. The speed of the centrifuge is 2500-3500r / min, the temperature in the fiber forming hood is 55-70°C, and the relative humidity is 22%-45%.

[0051] The molar ratio of the added amount of anhydrous aluminum chloride and aluminum powder is 1.7:2.1, preferably 1.8:2.0.

[0052] The second oxide phase is one of MgO, B2O3, Y2O3, and ZrO2, and the precursor sols are magnesium acetate solution, boric acid solution, yttrium acetate solution, and zirconium acetate solution, respectively.

[0053] The volume ratio of tetraethoxysilane, anhydrous ethanol, concentrated nitric acid, acetic acid and water is 10:5:1:1:15.

[0054] The process of heat treatment of the gel fiber in step five is as follows: put the gel fiber into a heat treatment furnace, heat it from 100°C to 600°C at a rate of 1.5°C / min, and keep it warm for 1 hour, wherein water vapor is introduced at 200-500°C to remove the acidic volatile gas produced by fiber pyrolysis, so that the fiber surface is not corroded; then heat it to 700°C at a rate of 3°C / min, and keep it warm for 1 hour; finally, heat the fiber to above 1300°C at 5°C / min, and keep it warm for 2 hours to obtain the mullite fiber to be prepared.

[0055] Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field and related fields without creative work should fall within the scope of protection of the present invention. The structures, devices and operating methods not specifically described and explained in the present invention are implemented according to the conventional means in the field unless otherwise specified and limited.

Claims

1. A toughened mullite ceramic, characterized in that: The invention is composed of the following parts by weight: 80-120 parts by weight of ceramic green body, 20-40 parts by weight of kaolinite, 8-20 parts by weight of hydromuscovite, 4-8 parts by weight of mullite fiber, 6-12 parts by weight of alumina particles, 14-24 parts by weight of attapulgite and 6-12 parts by weight of graphene.

2. The toughened mullite ceramic according to claim 1, characterized in that: The invention is composed of the following parts by weight: 100 parts by weight of ceramic green body, 30 parts by weight of kaolinite, 14 parts by weight of hydromuscovite, 6 parts by weight of mullite fiber, 9 parts by weight of alumina particles, 19 parts by weight of attapulgite and 9 parts by weight of graphene.

3. The toughened mullite ceramic according to claim 1, characterized in that: The ceramic blank is composed of the following parts by weight: 20-60 parts by weight of lithium mica tailings, 20-40 parts by weight of wollastonite tailings, 16-36 parts by weight of clay, 5-20 parts by weight of potassium feldspar, 5-20 parts by weight of sodium feldspar and 4-16 parts by weight of quartz.

4. A method for preparing toughened mullite ceramics, characterized in that: The following steps are included: Step 1: crushing kaolinite, quartz, hydromucovite, attapulgite and graphene, sieving the crushed kaolinite, quartz, hydromucovite, attapulgite and graphene, and reserving the sieved powder for later use; Step 2: mixing the sieved powder with mullite fibers and alumina particles, and ball milling the mixture using a ball mill, and setting the milled powder aside; Step 3: mixing the ball-milled powder with the ceramic blank, and adding an appropriate amount of tap water to the mixture to obtain a mixture; Step 4: The mixture is made into pottery through conventional embryo pulling, embryo drying and kiln firing processes.

5. The method for preparing toughened mullite ceramics according to claim 4, characterized in that: The method for preparing the ceramic blank comprises the following steps: Step 1: Prepare materials by weight, including lithium mica tailings, wollastonite tailings, clay, potassium feldspar, sodium feldspar, and quartz; Step 2: crush and screen the prepared mica tailings, wollastonite tailings, clay, potassium feldspar, sodium feldspar and quartz for later use; Step 3: Mix the mica tailings, wollastonite tailings, clay, potassium feldspar, sodium feldspar and quartz screened in step 2 to obtain a mixed blank; Step 4: wet ball milling the mixed blank to obtain blank slurry; Step 5: removing iron from the green body slurry and spray drying it to obtain a ceramic green body.

6. The method for preparing toughened mullite ceramics according to claim 4, characterized in that: The method for preparing the mullite fiber comprises the following steps: Step 1: Add aluminum chloride solution and aluminum powder in proportion to a heating and reflux reactor, heat at 95-110°C for 1.5-3h, and after the reaction is complete, filter to obtain a pale transparent polyaluminum chloride mother liquor; Step 2: adding a blend of tetraethoxysilane and anhydrous ethanol to a mixed solution of nitric acid and acetic acid, stirring for 0.8 h, the tetraethoxysilane is hydrolyzed to obtain a silicic acid solution; Step 3: adding the obtained silicic acid solution to the polyaluminium chloride mother liquor, adding acetic acid as a stabilizer and a spinning aid or other oxide second phase precursor sol, vacuum concentrating at 70-80° C. to obtain a mullite fiber precursor sol having a viscosity of 15-35 Pa·s; Step 4: centrifugal spinning is performed using a homemade centrifugal spinning machine to finally obtain gel fibers with uniform diameter; Step 5: Dry the obtained gel fiber at 50-70°C for 24 hours, and heat treat at 950-1500°C for 2 hours to obtain the desired mullite fiber.

7. The method for preparing toughened mullite ceramics according to claim 6, characterized in that: The centrifugal spinning process in step 4 is as follows: the precursor sol is centrifugally spun out from a small hole with an aperture of 0.45 mm at high speed under the action of centrifugal force, and then is pulled for a second time by a hot air flow of 50-70°C, dried and cured, and finally a precursor long fiber with uniform diameter and good toughness is obtained. The fiber length is 35-70cm and the diameter is 10-20um. Among them, the spinning head has a diameter of 50mm and a height of 40mm, and 16 small holes with a diameter of 0.45mm are evenly distributed around it. The rotation speed of the centrifuge is 2500-3500r / min, the temperature in the fiber forming hood is 55-70°C, and the relative humidity is 22%-45%.

8. The method for preparing toughened mullite ceramics according to claim 6, characterized in that: The molar ratio of the anhydrous aluminum chloride to the aluminum powder is 1.7:2.1, preferably 1.8:2.

0.

9. The method for preparing toughened mullite ceramics according to claim 6, characterized in that: The second oxide phase is one of MgO, B2O3, Y2O3, and ZrO2, and the precursor sols are magnesium acetate solution, boric acid solution, yttrium acetate solution, and zirconium acetate solution, respectively.

10. The method for preparing toughened mullite ceramics according to claim 6, characterized in that: The volume ratio of tetraethoxysilane, anhydrous ethanol, concentrated nitric acid, acetic acid and water is 10:5:1:1:15.

Citation Information

Patent Citations

  • Preparation method of mullite fiber

    CN104086200A

  • Mullite fiber toughened pot clay for pottery

    CN107555958A

  • Ceramic green body, ceramic tile and preparation method of ceramic green body

    CN115893978A