Low-linewidth low-temperature sintering gyromagnetic ferrite phase shifter substrate and preparation method thereof
By replacing Fe3+ ions into Bi3+ in NiCuZn ferrite and doping nano LiZn, low-line width low-temperature sintered rotary ferrite substrate is prepared, which solves the problem of poor density of traditional ferrite materials under low temperature sintering, and achieves low density Loss and high-performance microwave phase shifter substrate suitable for 5G/6G communication and active phased array radar.
Patent Information
- Application Number
- CN202410971219.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional ferrite materials have poor density under low temperature sintering, resulting in deterioration of rotary magnetic properties and increased losses, limiting the miniaturization and low loss development of microwave phase shifters.
The NiCuZn ferrite is used to replace Fe3+ ions as Bi3+ ions, combined with nano LiZn doping, and low-linear width low-temperature sintered rotary magnetite substrate is prepared through hot press sintering process, adjust the sintering temperature and microstructure, and optimize the rotary magnetism performance.
It realizes the low line width and high density rotary magnetite substrate under low temperature sintering conditions, reduces the loss of microwave devices, and meets the needs of 5G/6G communication and active phased array radar.
Smart Images

Figure HDA0004953281360000011 
Figure HDA0004953281360000012 
Figure HDA0004953281360000021
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electronic materials, and in particular relates to a low-linewidth, low-temperature sintered spin-magnetic ferrite phase shifter substrate and a preparation method thereof. Background Art
[0002] With the rapid development of 5G / 6G wireless communication, microwave communication is rapidly developing in communication base stations, satellites, and radars in weapons and equipment. The expansion of operating frequency to the microwave band and the high integration of electronic equipment have put forward higher requirements on the size and comprehensive performance of microwave devices. In addition, the microwave propagation frequency is 20-30GHz higher than the low frequency. In order to ensure the coverage range, the system needs to significantly increase the number of antennas, which brings at least 10 times the integration increment of microwave phase shifters, greatly increasing the loss and area of the communication system. At the same time, the new generation of communication systems requires microwave phase shifters to develop in the direction of miniaturization, high performance and integration. Ferrite materials are matched with low temperature co-fired ceramics (LTCC) technology, providing an effective solution to the miniaturization problem of microwave ferrite phase shifters. For the design of microwave phase shifters, traditional ferrite materials, as the substrate of phase shifters, face the problem of increased loss at higher microwave band frequencies. In addition, LTCC technology requires that the ferrite co-firing temperature be lower than the melting point of the silver electrode (961°C). Traditional ferrite materials have poor density, insufficient growth momentum, and small grain size under low-temperature sintering, which will cause a series of bottleneck problems such as deterioration of the gyromagnetic properties of ferrite materials and increased losses, limiting the miniaturization of microwave ferrite devices. Traditional high-temperature sintered ferrites have good density, but cannot be miniaturized. Therefore, the problem of miniaturization and low loss of microwave phase shifters is the main reason that directly affects the comprehensive performance of modern radar and communication systems. The development of new high-performance, low-loss microwave phase shifter substrate materials is the key to solving the above problems. Among them, reducing the sintering temperature of gyromagnetic ferrite materials while maintaining low line width is a technical problem that needs to be solved urgently. Summary of the invention
[0003] In order to overcome the deficiencies of the prior art, the purpose of the present invention is to propose a low-linewidth, low-temperature sintered rotary magnetic ferrite phase shifter substrate and a preparation method thereof, in response to the demand problems faced by the background technology.
[0004] The low line width low temperature sintered spin ferrite phase shifter substrate material of the present invention is based on the use of Bi in NiCuZn ferrite. 3+ Ion substitution Fe 3+Ions are used to reduce the sintering temperature and adjust the gyromagnetic properties. At the same time, in order to further obtain a lower line width, nano-LiZn ferrite is doped to further optimize the ferromagnetic resonance line width of NiCuZn ferrite. In the application of microwave devices, the low-linewidth gyromagnetic ferrite substrate can reduce the microwave loss of microwave devices, meet the wide application needs of microwave phase shifters in 5G / 6G communication base stations and active phased array radars, and further promote the progress of electronic technology and information technology.
[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0006] A low-linewidth, low-temperature sintered spin-magnetic ferrite phase shifter substrate and a preparation method thereof, characterized in that the ferrite material is Ni 0.18 Cu 0.2 Zn 0.62 Bi 0.02 Fe 1.98 O 4 -Nano-LiZn spinel ferrite (hereinafter referred to as NiCuZnBi-nano-LiZn) material is used to prepare a gyromagnetic ferrite phase shifter substrate with low ferromagnetic resonance linewidth and low temperature sintering by hot pressing sintering process.
[0007] The low-linewidth, low-temperature sintered spin-magnetic ferrite phase shifter substrate is based on the use of Bi in NiCuZn ferrite. 3+ Ion substitution Fe 3+ ions, low line width control under low temperature sintering, low line width substrate in microwave device application, increase the working area of the device, directly reduce the loss of microwave devices. Low temperature sintering can match LTCC process and realize the integration of microwave devices. 3+ Ion substitution Fe 3+ ions, obtain microwave characteristics with low line width, due to Bi 2 O 3 It has the effect of reducing the sintering temperature of ferrite, so Bi 3+ Substituting Fe in NiCuZn ferrite 3+ To reduce the sintering temperature of spinel ferrite; further, by adding different contents of nano-LiZn ferrite, the microstructure of NiCuZnBi ferrite is optimized to improve the degree of densification. The ferrite substrate material is prepared by hot pressing sintering. In the process, by applying different pressures and sintering temperature processes, low-linewidth low-temperature sintered spin-magnetic ferrite materials are prepared to meet the requirements of phase shifter substrate materials.
[0008] A low-linewidth, low-temperature sintered spin-magnetic ferrite phase shifter substrate and a preparation method thereof, characterized in that the preparation method comprises the following steps:
[0009] Step 1: Follow Ni0.18 Cu 0.2 Zn 0.62 Bi 0.02 Fe 1.98 O 4 The reactants are weighed in the stoichiometric ratio of NiCuZnBi, which are nickel oxide (NiO), copper oxide (CuO), zinc oxide (ZnO), and bismuth oxide (Bi 2 O 3 ), and ferric oxide (Fe 2 O 3 );
[0010] Step 2: Weigh the raw materials in step 1 according to the stoichiometric ratio to prepare the sintered powder of NiCuZnBi ferrite. The specific process is as follows:
[0011] 2.1 Place the weighed raw materials in a nylon ball mill, use zirconium oxide and deionized water as grinding media, and perform a one-time ball milling process. The ball milling time is 4-8 hours, and the speed is 220-280 rpm. After taking out, dry it in a blast drying oven;
[0012] 2.2 Pre-sinter the dried powder obtained in step 2.1 in a high temperature furnace at a temperature of 860-890°C for 2-4 hours to obtain NiCuZnBi ferrite pre-sintered powder;
[0013] Step 3: Preparation of nano-LiZn. The specific process is as follows:
[0014] 3.1 According to Li 0.361 Zn 0.26 Fe 2.367 O 4 The reactants are weighed in a stoichiometric ratio. The reactant is lithium nitrate (LiNO 3 ), zinc nitrate (Zn(NO 3 ) 2 6H 2 O,), ferric nitrate (Fe(NO 3 ) 3 6H 2 O), sodium hydroxide (NaOH), dissolve it in deionized water, stir it with a magnetic stirrer, and set the temperature of the magnetic stirrer to 15°C-35°C to titrate the sodium hydroxide solution to adjust the pH value to 8-10;
[0015] 3.2 After the titration is completed, transfer the mixture to an ultrasonic cleaner and sonicate for 20-40 minutes;
[0016] 3.3 Let it stand for 10-20 minutes and transfer the mixture to the reactor. The starting temperature of the reactor is set to 20℃-25℃ at room temperature, the maximum temperature is set to 180℃-280℃, the heating rate is 1-2℃ / minute, the speed of the reactor is uniformly 180-220 rpm, and the insulation time is 5 hours to 40 hours. After the heating and insulation time is reached, turn off the heating and keep the motor running continuously to maintain the uniformity of the reactants during the cooling period. After cooling to room temperature, take out the material for suction filtration, wash until the pH is close to 7, and then add anhydrous ethanol to wash once to ensure the dispersion and purity of the material;
[0017] 3.4 The material is transferred to an oven for drying, and then ground into powder to obtain nano-LiZn powder;
[0018] Step 4, the NiCuZnBi ferrite pre-sintered powder obtained in step 2 and the nano-LiZn powder obtained in step 3 are loaded into a ball mill according to NiCuZnBi-x nano-LiZn ferrite (wherein x=2.0wt% to 8wt%), and zirconium oxide and deionized water are added as grinding media, and secondary ball milling is performed, the ball milling time is 8-12 hours, the speed is 220-250 rpm, and after the ball milling is completed, it is taken out and dried in a blast drying oven to obtain a dried low line width NiCuZnBi-nano-LiZn powder;
[0019] Step 5: Using the hot pressing sintering process, the sintered powder obtained in step 4 is placed in a hot pressing sintering mold, pressurized at 20 MPa-60 MPa, heated at a rate of 1-2°C / min, and sintered at a temperature of 850-940°C, then taken out and tested.
[0020] The present invention also provides the application of the low-temperature sintered spin-magnetic ferrite phase shifter substrate with low line width as a microwave phase shifter.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The present invention provides a low-linewidth, low-temperature sintered spin-magnetic ferrite phase shifter substrate, the material formula of which is Ni 0.18 Cu 0.2 Zn 0.62 Bi 0.02 Fe 1.98 O 4 Spinel ferrite material, through Bi 3+ Ion substitution achieves low-temperature sintering of NiCuZn ferrite and microstructure densification regulation under low-temperature sintering. The second ball milling uses nano-LiZn additives to further regulate the gyromagnetic properties of ferrite materials under low-temperature sintering, and prepares spinel-type gyromagnetic ferrite phase shifter substrates with low-temperature sintering and low line width to meet the application requirements of microwave phase shifters.
[0023] 2. The present invention provides a low-linewidth, low-temperature sintered gyromagnetic ferrite phase shifter substrate, which has the characteristics of high remanence ratio, high saturation magnetization intensity and low ferromagnetic resonance linewidth under low-temperature sintering. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a flowchart of the method for preparing a low-linewidth, low-temperature sintered spin-magnetic ferrite phase shifter substrate material according to the present invention.
[0025] Figure 2 This is a comparison of scanning electron microscope images (SEM) of low-linewidth, low-temperature sintered spin-magnetic ferrite phase shifter substrate materials of Example 3 and Example 1 of the present invention.
[0026] Figure 3 1 is the XRD diagram of the low-linewidth, low-temperature sintered rotary magnetic ferrite phase shifter substrate material of Examples 1, 2, 3 and 4 of the present invention.
[0027] Figure 4 Graph showing the ferromagnetic resonance (FMR) linewidth fitting spectrum (Lorentz fitting) of the low-linewidth, low-temperature sintered gyromagnetic ferrite phase shifter substrate materials of Examples 1, 2, 3 and 4 of the present invention.
[0028] Figure 5 The saturation magnetization intensity diagram of the low-linewidth, low-temperature sintered rotary magnetic ferrite phase shifter substrate material of Examples 1, 2, 3 and 4 of the present invention. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is described in detail below in conjunction with the accompanying drawings and embodiments.
[0030] Example 1
[0031] A low-linewidth, low-temperature sintered spin-magnetic ferrite phase shifter substrate and a preparation method thereof, characterized in that the preparation method comprises the following steps:
[0032] Step 1: Follow Ni 0.18 Cu 0.2 Zn 0.62 Bi 0.02 Fe 1.98 O 4 The reactants are weighed in the stoichiometric ratio of (referred to as NiCuZnBi), the reactants are nickel oxide (NiO) 2.69g, copper oxide (CuO) 3.18g, zinc oxide (ZnO) 10.10g, bismuth oxide (Bi 2 O 3 ) is 1.86g, and ferric oxide (Fe 2 O 3 ) is 31.62g;
[0033] Step 2: Weigh the raw materials in step 1 according to the stoichiometric ratio to prepare the sintered powder of NiCuZnBi ferrite. The specific process is as follows:
[0034] 2.2 Place the weighed raw materials in a nylon ball mill, use zirconium oxide and deionized water as grinding media, and perform a one-time ball milling process. The ball milling time is 6 hours, the speed is 250 rpm, and the raw materials are taken out and dried in a blast drying oven;
[0035] 2.2 The dried powder obtained in step 2.1 is pre-sintered in a high temperature furnace at a temperature of 880° C. for 3 hours to obtain NiCuZnBi ferrite pre-sintered powder;
[0036] Step 3: Preparation of nano-LiZn. The specific process is as follows:
[0037] 3.1 According to Li 0.361 Zn 0.26 Fe 2.367 O 4 The reactants are weighed in a stoichiometric ratio. The reactant is lithium nitrate (LiNO 3 ), zinc nitrate (Zn(NO 3 ) 2 6H 2 O,), ferric nitrate (Fe(NO 3 ) 3 6H 2 O), sodium hydroxide (NaOH), dissolved in deionized water, stirred with a magnetic stirrer, and the temperature of the magnetic stirrer was set to 25 ° C to titrate the sodium hydroxide solution to adjust the pH value to 9;
[0038] 3.2 After the titration is completed, transfer the mixture to an ultrasonic cleaner and sonicate for 30 minutes;
[0039] 3.3 Let the mixture stand for 10-20 minutes and transfer it to the reactor. The starting temperature of the reactor is set to 22°C at room temperature, the maximum temperature is set to 220°C, the heating rate is 2°C / minute, the speed of the reactor is uniformly set to 200 rpm, and the insulation time is 20 hours. After the heating and insulation time is reached, turn off the heating and keep the motor running continuously to maintain the uniformity of the reactants during the cooling period. After cooling to room temperature, take out the material for suction filtration, wash until the pH is close to 7, and then add anhydrous ethanol for washing once to ensure the dispersion and purity of the material;
[0040] 3.4 The material is transferred to an oven for drying, and then ground into powder to obtain nano-LiZn powder;
[0041] Step 4, the NiCuZnBi ferrite pre-sintered powder obtained in step 2 and the nano-LiZn powder obtained in step 3 are loaded into a ball mill according to NiCuZnBi-2.0wt% nano-LiZn ferrite, and zirconium oxide and deionized water are added as grinding media, and secondary ball milling is performed, the ball milling time is 12 hours, the speed is 220 rpm, and the ball milling is taken out after the ball milling is completed, and dried in a blast drying oven to obtain a dried low line width NiCuZnBi-nano-LiZn powder;
[0042] Step 5: Using the hot pressing sintering process, the sintered powder obtained in step 4 is placed in a hot pressing sintering mold, pressurized to 48 MPa, heated at a rate of 2°C / min, and sintered at 920°C, then taken out and tested.
[0043] The NiCuZnBi microwave ferrite substrate material was tested by BH analyzer, XRD test, SEM test, vibration magnetometer, and FMR line width (ΔH) test of the sample at 9.56GHz using TE106 perturbation method. The results are as follows:
[0044] Remanence ratio M r / M s : 0.76; saturation magnetization: 51.5emu / g; ferromagnetic resonance linewidth: 189Oe.
[0045] Example 2
[0046] A low-linewidth, low-temperature sintered spin-magnetic ferrite phase shifter substrate and a preparation method thereof, specifically comprising the following steps:
[0047] Step 1: Follow Ni 0.18 Cu 0.2 Zn 0.62 Bi 0.02 Fe 1.98 O 4 The reactants are weighed in the stoichiometric ratio of (referred to as NiCuZnBi), the reactants are nickel oxide (NiO) 2.69g, copper oxide (CuO) 3.18g, zinc oxide (ZnO) 10.10g, bismuth oxide (Bi 2 O 3 ) is 1.86g, and ferric oxide (Fe 2 O 3 ) is 31.62g;
[0048] Step 2: Weigh the raw materials in step 1 according to the stoichiometric ratio to prepare the sintered powder of NiCuZnBi ferrite. The specific process is as follows:
[0049] 2.3 Place the weighed raw materials in a nylon ball mill, use zirconium oxide and deionized water as grinding media, and perform a one-time ball milling process. The ball milling time is 6 hours, the speed is 250 rpm, and the raw materials are taken out and dried in a blast drying oven;
[0050] 2.2 The dried powder obtained in step 2.1 is pre-sintered in a high temperature furnace at a temperature of 880° C. for 3 hours to obtain NiCuZnBi ferrite pre-sintered powder;
[0051] Step 3: Preparation of nano-LiZn. The specific process is as follows:
[0052] 3.1 According to Li 0.361 Zn 0.26 Fe 2.367 O 4 The reactants are weighed in a stoichiometric ratio. The reactant is lithium nitrate (LiNO 3 ), zinc nitrate (Zn(NO 3 ) 2 6H 2 O,), ferric nitrate (Fe(NO 3 ) 3 6H 2 O), sodium hydroxide (NaOH), dissolved in deionized water, stirred with a magnetic stirrer, and the temperature of the magnetic stirrer was set to 25 ° C to titrate the sodium hydroxide solution to adjust the pH value to 9;
[0053] 3.2 After the titration is completed, transfer the mixture to an ultrasonic cleaner and sonicate for 30 minutes;
[0054] 3.3 Let the mixture stand for 10-20 minutes and transfer it to the reactor. The starting temperature of the reactor is set to 22°C at room temperature, the maximum temperature is set to 220°C, the heating rate is 2°C / minute, the speed of the reactor is uniformly set to 200 rpm, and the insulation time is 20 hours. After the heating and insulation time is reached, turn off the heating and keep the motor running continuously to maintain the uniformity of the reactants during the cooling period. After cooling to room temperature, take out the material for suction filtration, wash until the pH is close to 7, and then add anhydrous ethanol for washing once to ensure the dispersion and purity of the material;
[0055] 3.4 The material is transferred to an oven for drying, and then ground into powder to obtain nano-LiZn powder;
[0056] Step 4, the NiCuZnBi ferrite pre-sintered powder obtained in step 2 and the nano-LiZn powder obtained in step 3 are loaded into a ball mill according to NiCuZnBi-4.0wt% nano-LiZn ferrite, and zirconium oxide and deionized water are added as grinding media, and secondary ball milling is performed, the ball milling time is 12 hours, the speed is 220 rpm, and the ball milling is taken out after the ball milling is completed, and dried in a blast drying oven to obtain a dried low line width NiCuZnBi-nano-LiZn powder;
[0057] Step 5: Using the hot pressing sintering process, the sintered powder obtained in step 4 is placed in a hot pressing sintering mold, pressurized to 48 MPa, heated at a rate of 2°C / min, and sintered at 920°C, then taken out and tested.
[0058] The NiCuZnBi microwave ferrite substrate material was tested by BH analyzer, XRD test, SEM test, vibration magnetometer, and FMR line width (ΔH) test of the sample at 9.56GHz using TE106 perturbation method. The results are as follows:
[0059] The NiCuZnBi microwave ferrite substrate material was tested by BH analyzer, XRD test, SEM test, vibration magnetometer, and FMR line width (ΔH) test of the sample at 9.56GHz using TE106 perturbation method. The results are as follows:
[0060] Remanence ratio M r / M s :0.81;Saturation magnetization: 53.9emu / g;Ferromagnetic resonance linewidth: 164Oe;
[0061] Example 3
[0062] A low-linewidth, low-temperature sintered spin-magnetic ferrite phase shifter substrate and a preparation method thereof, specifically comprising the following steps:
[0063] Step 1: Follow Ni 0.18 Cu 0.2 Zn 0.62 Bi 0.02 Fe 1.98 O 4 The reactants are weighed in the stoichiometric ratio of (referred to as NiCuZnBi), the reactants are nickel oxide (NiO) 2.69g, copper oxide (CuO) 3.18g, zinc oxide (ZnO) 10.10g, bismuth oxide (Bi 2 O 3 ) is 1.86g, and ferric oxide (Fe 2 O 3 ) is 31.62g;
[0064] Step 2: Weigh the raw materials in step 1 according to the stoichiometric ratio to prepare the sintered powder of NiCuZnBi ferrite. The specific process is as follows:
[0065] 2.4 Place the weighed raw materials in a nylon ball mill, use zirconium oxide and deionized water as grinding media, and perform a one-time ball milling process. The ball milling time is 6 hours, the speed is 250 rpm, and the raw materials are taken out and dried in a blast drying oven;
[0066] 2.2 The dried powder obtained in step 2.1 is pre-sintered in a high temperature furnace at a temperature of 880° C. for 3 hours to obtain NiCuZnBi ferrite pre-sintered powder;
[0067] Step 3: Preparation of nano-LiZn. The specific process is as follows:
[0068] 3.1 According to Li 0.361 Zn 0.26 Fe 2.367 O 4 The reactants are weighed in a stoichiometric ratio. The reactant is lithium nitrate (LiNO 3 ), zinc nitrate (Zn(NO 3 ) 2 6H 2 O,), ferric nitrate (Fe(NO 3 ) 3 6H 2 O), sodium hydroxide (NaOH), dissolved in deionized water, stirred with a magnetic stirrer, and the temperature of the magnetic stirrer was set to 25 ° C to titrate the sodium hydroxide solution to adjust the pH value to 9;
[0069] 3.2 After the titration is completed, transfer the mixture to an ultrasonic cleaner and sonicate for 30 minutes;
[0070] 3.3 Let the mixture stand for 10-20 minutes and transfer it to the reactor. The starting temperature of the reactor is set to 22°C at room temperature, the maximum temperature is set to 220°C, the heating rate is 2°C / minute, the speed of the reactor is uniformly set to 200 rpm, and the insulation time is 20 hours. After the heating and insulation time is reached, turn off the heating and keep the motor running continuously to maintain the uniformity of the reactants during the cooling period. After cooling to room temperature, take out the material for suction filtration, wash until the pH is close to 7, and then add anhydrous ethanol for washing once to ensure the dispersion and purity of the material;
[0071] 3.4 The material is transferred to an oven for drying, and then ground into powder to obtain nano-LiZn powder;
[0072] Step 4, the NiCuZnBi ferrite pre-sintered powder obtained in step 2 and the nano-LiZn powder obtained in step 3 are loaded into a ball mill according to NiCuZnBi-6.0wt% nano-LiZn ferrite, and zirconium oxide and deionized water are added as grinding media, and secondary ball milling is performed, the ball milling time is 12 hours, the speed is 220 rpm, and after the ball milling is completed, the powder is taken out and dried in a blast drying oven to obtain a dried low line width NiCuZnBi-nano-LiZn powder;
[0073] Step 5: Using the hot pressing sintering process, the sintered powder obtained in step 4 is placed in a hot pressing sintering mold, pressurized to 48 MPa, heated at a rate of 2°C / min, and sintered at 920°C, then taken out and tested.
[0074] The NiCuZnBi microwave ferrite substrate material was tested by BH analyzer, XRD test, SEM test, vibration magnetometer, and FMR line width (ΔH) test of the sample at 9.56GHz using TE106 perturbation method. The results are as follows:
[0075] Remanence ratio M r / M s : 0.89; saturation magnetization: 58.6emu / g; ferromagnetic resonance linewidth: 135Oe.
[0076] Example 4
[0077] A low-linewidth, low-temperature sintered spin-magnetic ferrite phase shifter substrate and a preparation method thereof, specifically comprising the following steps:
[0078] Step 1: Follow Ni 0.18 Cu 0.2 Zn 0.62 Bi 0.02 Fe 1.98 O 4 The reactants are weighed in the stoichiometric ratio of (referred to as NiCuZnBi), the reactants are nickel oxide (NiO) 2.69g, copper oxide (CuO) 3.18g, zinc oxide (ZnO) 10.10g, bismuth oxide (Bi 2 O 3 ) is 1.86g, and ferric oxide (Fe 2 O 3 ) is 31.62g;
[0079] Step 2: Weigh the raw materials in step 1 according to the stoichiometric ratio to prepare the sintered powder of NiCuZnBi ferrite. The specific process is as follows:
[0080] 2.5 Place the weighed raw materials in a nylon ball mill, use zirconium oxide and deionized water as grinding media, and perform a one-time ball milling process. The ball milling time is 6 hours, the speed is 250 rpm, and the raw materials are taken out and dried in a blast drying oven;
[0081] 2.2 The dried powder obtained in step 2.1 is pre-sintered in a high temperature furnace at a temperature of 880° C. for 3 hours to obtain NiCuZnBi ferrite pre-sintered powder;
[0082] Step 3: Preparation of nano-LiZn. The specific process is as follows:
[0083] 3.1 According to Li 0.361 Zn 0.26 Fe 2.367 O 4 The reactants are weighed in a stoichiometric ratio. The reactant is lithium nitrate (LiNO 3 ), zinc nitrate (Zn(NO 3 ) 2 6H 2 O,), ferric nitrate (Fe(NO 3 ) 3 6H 2 O), sodium hydroxide (NaOH), dissolved in deionized water, stirred with a magnetic stirrer, and the temperature of the magnetic stirrer was set to 25 ° C to titrate the sodium hydroxide solution to adjust the pH value to 9;
[0084] 3.2 After the titration is completed, transfer the mixture to an ultrasonic cleaner and sonicate for 30 minutes;
[0085] 3.3 Let the mixture stand for 10-20 minutes and transfer it to the reactor. The starting temperature of the reactor is set to 22°C at room temperature, the maximum temperature is set to 220°C, the heating rate is 2°C / minute, the speed of the reactor is uniformly set to 200 rpm, and the insulation time is 20 hours. After the heating and insulation time is reached, turn off the heating and keep the motor running continuously to maintain the uniformity of the reactants during the cooling period. After cooling to room temperature, take out the material for suction filtration, wash until the pH is close to 7, and then add anhydrous ethanol for washing once to ensure the dispersion and purity of the material;
[0086] 3.4 The material is transferred to an oven for drying, and then ground into powder to obtain nano-LiZn powder;
[0087] Step 4, the NiCuZnBi ferrite pre-sintered powder obtained in step 2 and the nano-LiZn powder obtained in step 3 are loaded into a ball mill according to NiCuZnBi-8.0wt% nano-LiZn ferrite, and zirconium oxide and deionized water are added as grinding media, and secondary ball milling is performed, the ball milling time is 12 hours, the speed is 220 rpm, and after the ball milling is completed, it is taken out and dried in a blast drying oven to obtain a dried low line width NiCuZnBi-nano-LiZn powder;
[0088] Step 5: Using the hot pressing sintering process, the sintered powder obtained in step 4 is placed in a hot pressing sintering mold, pressurized to 48 MPa, heated at a rate of 2°C / min, and sintered at 920°C, then taken out and tested.
[0089] The NiCuZnBi microwave ferrite substrate material was tested by BH analyzer, XRD test, SEM test, vibration magnetometer, and FMR line width (ΔH) test of the sample at 9.56GHz using TE106 perturbation method. The results are as follows:
[0090] Remanence ratio M r / M s : 0.83; saturation magnetization: 52.1emu / g; ferromagnetic resonance linewidth: 154Oe.
[0091] Figure 2 This is a scanning electron microscope (SEM) comparison of low-temperature sintered spin-magnetic ferrite phase shifter substrate materials with low line widths in Example 3 and Example 1 of the present invention. Figure 2 It can be seen that the NiCuZnBi ferrite grains obtained by adding 6wt% nano-LiZn in Example 3 are further grown, and the grain growth is more dense and uniform, and no abnormal grains appear.
[0092] Figure 3 XRD patterns of low-temperature sintered ferrite phase shifter substrates with low line width prepared in Examples 1, 2, 3 and 4 of the present invention. It can be seen from the figure that the basic phase of the substrate is a single spinel ferrite material structure without other impurities, and the XRD pattern of the substrate becomes smoother with the change of nano-LiZn content.
[0093] Figure 4 The ferromagnetic resonance (FMR) line width fitting spectrum (Lorentz fitting) of the low line width, low temperature sintered gyromagnetic ferrite phase shifter substrate material of Examples 1, 2, 3 and 4 of the present invention is shown. Figure 4It can be seen that the fitted Lorentz spectrum is very consistent with the experimental result, and the FMR line width value can be obtained from the FMR line width fitting spectrum. Obviously, adding appropriate nano-LiZn effectively reduces the FMR line width value. Compared with Example 1 (no nano-LiZn is added), the NiCuZnBi ferrite obtained when 6wt% nano-LiZn is added in Example 3 has the lowest FMR line width value of 135Oe.
[0094] Figure 5 is the saturation magnetization intensity (M) of the low-linewidth, low-temperature sintered spin-magnetic ferrite phase shifter substrate material of Examples 1, 2, 3 and 4 of the present invention. s ) Figure, by Figure 5 It can be seen that the saturation magnetization intensities of Examples 1, 2, 3 and 4 have all changed. Compared with Example 1, M s Therefore, adding nano-LiZn can effectively increase the saturation magnetization intensity. The maximum saturation magnetization intensity M is obtained in Comparative Example 3. s =58.6emu / g.
[0095] The remanence ratio, saturation magnetization, and ferromagnetic resonance line width test data results of the low-temperature sintered gyromagnetic ferrite phase shifter substrate material with low line width obtained in Examples 1, 2, 3, and 4. The remanence ratio of the substrate increases from 0.76 to 0.89 with the addition of appropriate nano-LiZn content, indicating that the magnetic field orientation of the garnet ferrite substrate gradually becomes consistent, which improves the remanence ratio and has a self-bias effect. At the same time, the saturation magnetization M s The FMR increased from 51.5emu / g to 58.6emu / g, and decreased from 189Oe to 135Oe, indicating that the substrate has high gyromagnetic properties while maintaining low-temperature sintering characteristics. From the perspective of ferromagnetic resonance line width, a very low FMR was obtained, indicating that the substrate has low microwave loss.
[0096] According to the results, the low-temperature sintered gyromagnetic ferrite phase shifter substrate with low line width of the embodiment has a higher remanence ratio, saturation magnetization intensity, and low ferromagnetic resonance line width under low-temperature sintering, and can be used as a gyromagnetic ferrite phase shifter substrate material.
[0097] The above embodiments are only preferred implementations of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A low-linewidth, low-temperature sintered spin-magnetic ferrite phase shifter substrate and a preparation method thereof, It is characterized in that The ferrite material is Ni 0.18 Cu 0.2 Zn 0.62 Bi 0.02 Fe 1.98 O 4 -Nano-LiZn spinel ferrite (hereinafter referred to as NiCuZnBi-nano-LiZn) material is used to prepare a low-linewidth, low-temperature sintered spino-magnetic ferrite phase shifter substrate by hot pressing and sintering process.
2. A low line width, low temperature sintered spin-magnetic ferrite phase shifter substrate according to claim 1, It is characterized in that The low-linewidth, low-temperature sintered spin-magnetic ferrite phase shifter substrate is based on the use of Bi in NiCuZn ferrite. 3+ Ion substitution Fe 3+ ions, low line width control under low temperature sintering, low line width substrate in microwave device application, increase the working area of the device, directly reduce the loss of microwave devices. Low temperature sintering can match LTCC process and realize the integration of microwave devices; using Bi 3+ Ion substitution Fe 3+ ions, obtain microwave characteristics with low line width, due to Bi 2 O 3 It has the effect of reducing the sintering temperature of ferrite, so Bi 3+ Substituting Fe in NiCuZn ferrite 3+ To reduce the sintering temperature of spinel ferrite; further, the microstructure of NiCuZnBi ferrite is optimized by adding different contents of nano-LiZn ferrite to improve the degree of densification; the ferrite substrate material is prepared by hot pressing sintering, and by applying different pressures and sintering temperatures in the process, a low-linewidth, low-temperature sintered spin-magnetic ferrite material is prepared to meet the requirements of phase shifter substrate materials.
3. A low-linewidth, low-temperature sintered spin-magnetic ferrite phase shifter substrate and a preparation method thereof according to claim 1, It is characterized in that The preparation method comprises the following steps: Step 1: Follow Ni 0.18 Cu 0.2 Zn 0.62 Bi 0.02 Fe 1.98 O 4 The reactants are weighed in the stoichiometric ratio of NiCuZnBi, which are nickel oxide (NiO), copper oxide (CuO), zinc oxide (ZnO), and bismuth oxide (Bi 2 O 3 ), and ferric oxide (Fe 2 O 3 ); Step 2: Weigh the raw materials in step 1 according to the stoichiometric ratio to prepare the sintered powder of NiCuZnBi ferrite. The specific process is as follows: 2.1 Place the weighed raw materials in a nylon ball mill, use zirconium oxide and deionized water as grinding media, and perform a one-time ball milling process. The ball milling time is 4-8 hours, and the speed is 220-280 rpm. After taking out, dry it in a blast drying oven; 2.2 Pre-sinter the dried powder obtained in step 2.1 in a high temperature furnace at a temperature of 860-890°C for 2-4 hours to obtain NiCuZnBi ferrite pre-sintered powder; Step 3: Preparation of nano-LiZn. The specific process is as follows: 3.1 According to Li 0.361 Zn 0.26 Fe 2.367 O 4 The reactants are weighed in a stoichiometric ratio. The reactant is lithium nitrate (LiNO 3 ), zinc nitrate (Zn(NO 3 ) 2 6H 2 O,), ferric nitrate (Fe(NO 3 ) 3 6H 2 O), sodium hydroxide (NaOH), dissolve it in deionized water, stir it with a magnetic stirrer, and set the temperature of the magnetic stirrer to 15°C-35°C to titrate the sodium hydroxide solution to adjust the pH value to 8-10; 3.2 After the titration is completed, transfer the mixture to an ultrasonic cleaner and sonicate for 20-40 minutes; 3.3 After standing for 10-20 minutes, transfer the mixture to the reactor. The starting temperature of the reactor is set to room temperature 20℃-25℃, the maximum temperature is set to 180℃-280℃, the heating rate is 1-2℃ / min, the speed of the reactor is uniformly 180-220 rpm, and the insulation time is 5 hours to 40 hours. After the heating and insulation time is reached, turn off the heating and keep the motor running continuously to maintain the uniformity of the reactants during the cooling period. After cooling to room temperature, take out the material for suction filtration, wash until the pH is close to 7, and then add anhydrous ethanol for washing once to ensure the dispersion and purity of the material; 3.4 The material is transferred to an oven for drying, and then ground into powder to obtain nano-LiZn powder; Step 4, the NiCuZnBi ferrite pre-sintered powder obtained in step 2 and the nano-LiZn powder obtained in step 3 are loaded into a ball mill according to NiCuZnBi-x nano-LiZn ferrite (wherein x=2.0wt% to 8wt%), and zirconium oxide and deionized water are added as grinding media, and secondary ball milling is performed, the ball milling time is 8-12 hours, the speed is 220-250 rpm, and after the ball milling is completed, it is taken out and dried in a blast drying oven to obtain a dried low line width NiCuZnBi-nano-LiZn powder; Step 5: Using the hot pressing sintering process, the sintered powder obtained in step 4 is placed in a hot pressing sintering mold, pressurized at 20 MPa-60 MPa, heated at a rate of 1-2°C / min, and sintered at a temperature of 850-940°C, then taken out and tested.
4. The low-linewidth, low-temperature sintered spin-magnetic ferrite substrate according to claim 1 or 2 is used as a substrate material for a phase shifter in a microwave device.
5. The method according to claim 3 obtains a low-linewidth, low-temperature sintered spin-magnetic ferrite phase shifter substrate.
Citation Information
Patent Citations
High performance low temperature sintered hexagonal M-type strontium ferrite and preparation method thereof
CN106187144A
NiCuZn gyromagnetic ferrite material for LTCC circulators and preparation method thereof
CN108774057A
Low-temperature-sintered low-loss LiZn ferrite material and preparation method
CN109053180A
Spinel Li-series ferrite material for x-band to millimeter wave-band lock phase shifter
CN109437879A
High-saturation low-temperature-sintered gyromagnetic Ni-series spinel ferrite material and preparation method thereof
CN112321291A