Spherical yttrium aluminum garnet powder and method for in-situ synthesis of spherical yttrium aluminum garnet powder through spray granulation technology

Through spray granulation technology, the in-situ synthesis of spherical YAG powder at low temperatures is solved, and the problem of high temperature and high cost in traditional methods is achieved, and the preparation of spherical YAG powder is achieved, which is suitable for large-scale industrial production.

CN118908712APending Publication Date: 2024-11-08SHANGHAI UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410971271.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the existing preparation methods for spherical yttrium aluminum garnet (YAG) powder, the liquid phase method requires a large amount of solvent and precipitant, with low yield and high synthesis temperature of traditional solid phase reaction method, resulting in high cost and reduced sintering activity, which limits the large amount of Large-scale production.

Method used

Spray granulation technology is used to synthesize spherical YAG powder in situ at low temperature, and mix slurry is prepared by mechanically stirring yttrium and alumina powder with dispersant and binder. The spray dryer is used to granulate and calcinate at low temperature under air atmosphere. , realize the preparation of spherical YAG powder.

Benefits of technology

It reduces preparation cost and energy consumption, improves the uniformity and fluidity of the powder, reduces the synthesis temperature, is suitable for large-scale industrial production, and realizes efficient YAG single-phase synthesis.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908712A_ABST
    Figure CN118908712A_ABST
Patent Text Reader

Abstract

The invention relates to the field of inorganic powder preparation, and provides a method for in-situ synthesis of spherical yttrium aluminum garnet powder through a spray granulation technology, and the method comprises the following steps: S1, mechanically stirring yttrium oxide (Y2O3) powder, aluminum oxide (Al2O3) powder, deionized water, a dispersant and a binder to obtain mixed slurry; s2, performing spray granulation on the mixed slurry to obtain spherical mixed powder; and S3, putting the spherical mixed powder into a muffle furnace, and carrying out pressureless calcination in an air atmosphere. The method is simple in process, low in cost and energy consumption, high in yield, free of environmental pollution and suitable for large-scale industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for synthesizing spherical yttrium aluminum garnet (YAG) powder in situ at low temperature by spray granulation technology and the synthesized spherical yttrium aluminum garnet powder. The powder is suitable for plasma spraying and ceramic pressing. Background Art

[0002] With the rapid development of science and technology, the demand for high-performance ceramics is increasing. As an important inorganic non-metallic material, yttrium aluminum garnet (YAG) is widely used in ceramics, coatings, electronics, medical and other fields due to its excellent optical, thermal and mechanical properties. In recent years, with the improvement of material performance requirements, spherical YAG powder has attracted widespread attention due to its unique physical and chemical properties: due to its unique spherical structure, the particle size distribution is relatively narrow, thus ensuring the uniformity of powder particles during the molding process. This high uniformity can greatly improve the accuracy and quality of material preparation and make the physical and chemical properties of the material to the best play; in addition, spherical YAG powder has good fluidity due to its regular particle shape, and there will be no particle staggering and accumulation, so it has excellent fluidity, making the production process more efficient. At the same time, the spherical structure can better fill the gaps in the molding mold, thereby improving the density of ceramics; finally, spherical YAG has a compact structure and high plasticity, which can more conveniently prepare various complex shapes of materials, and has higher physical and chemical properties, such as hardness and etching resistance. Therefore, the preparation technology of spherical YAG powder is of great significance to improving the technical level and market competitiveness of related industries.

[0003] The preparation methods of spherical YAG powder usually include liquid phase method and solid phase method. The preparation of spherical YAG powder by liquid phase method usually requires a large amount of solvent and precipitant, and the output is low, which increases the preparation cost and limits its application in large-scale production. The traditional solid phase reaction method usually causes the powder to lose its sintering activity due to the high synthesis temperature and long time. The solid phase reaction method of Y2O3 powder and Al2O3 powder usually requires a temperature higher than 1400℃ to effectively synthesize the YAG phase, and the pure phase requires a higher calcination temperature, usually 1600℃.

[0004] The Chinese patent with publication number CN 111925202B discloses a sintering-free yttrium aluminum garnet powder, yttrium aluminum garnet ceramics, and a preparation method and application thereof. The method spheroidizes YAG coarse powder in a fluidized bed to obtain spherical YAG powder with an average particle size of 10 μm to 300 μm. However, the particle size of fluidized bed granulation is relatively large, and multiple parameters need to be adjusted during operation, which has the disadvantages of high energy consumption and high cost. Summary of the invention

[0005] In order to solve or partially solve the above technical problems, the present invention provides a method for in-situ synthesis of spherical yttrium aluminum garnet powder by spray granulation technology, comprising the following steps:

[0006] S1, mechanically stirring yttrium oxide (Y2O3) powder, aluminum oxide (Al2O3) powder, deionized water, a dispersant, and a binder to obtain a mixed slurry;

[0007] S2, spray granulating the mixed slurry to obtain spherical mixed powder;

[0008] S3. placing the spherical mixed powder in a muffle furnace and calcining it without pressure in an air atmosphere.

[0009] Optionally, the mixed slurry preparation comprises the following steps:

[0010] S11, according to Y3Al5O 12 Yttrium oxide (Y2O3) powder, aluminum oxide (Al2O3) powder and deionized water are mechanically stirred and mixed in a stoichiometric ratio;

[0011] S12, after stirring for a period of time, add dispersant and continue stirring;

[0012] S13, adding a binder before granulation to obtain a mixed slurry.

[0013] Optionally, in step S11, the solid content of the mixed slurry is 30-60 wt.%.

[0014] Optionally, in step S12, the dispersant is selected from one of ammonium citrate, sodium hexametaphosphate, polyvinyl butyral, and polyvinyl pyrrolidone, and the added amount is 0.1 to 2 wt.% of the mass of the powder;

[0015] The binder is selected from one of polyvinyl alcohol and polyvinyl butyral, and the added amount is 0.1-1wt.% of the powder mass.

[0016] Optionally, in step S2, the mixed slurry is granulated by a spray dryer, the inlet temperature of the spray dryer is 150-300°C, and the outlet temperature is 50-200°C; the atomizer speed of the spray dryer is 30-50 Hz.

[0017] Optionally, in step S2, the particle size of the spherical mixed powder obtained by granulation is 10 to 100 μm.

[0018] Optionally, in step S2, the sphericity standard deviation of the spherical mixed powder obtained by granulation is 0 to 0.3.

[0019] Optionally, in step S2, the fluidity index of the spherical mixed powder obtained by granulation is 70-90.

[0020] Optionally, in step S3, the conditions of the calcination process are: a heating rate of 1 to 10°C / min; a calcination temperature range of 1000 to 1600°C; and a high temperature insulation time of 2 to 10 hours.

[0021] The present invention also provides a spherical yttrium aluminum garnet (YAG) powder, which is optionally synthesized by any of the above methods.

[0022] The present invention adopts micron-grade Y2O3 powder as raw material, and the refined Y2O3 powder and Al2O3 powder are mixed according to Y3Al5O 12 The stoichiometric ratio is set, and a dispersant and a binder are added to prepare a mixed slurry. The obtained slurry is sent to the inside of a spray dryer by a peristaltic pump to contact with hot air to achieve spray granulation. EDS scanning shows that the closer the molar ratio of Y element to Al element is to the stoichiometric ratio of 0.60, the better the dispersion uniformity is, which can reduce costs.

[0023] Specifically, the method adopts an Al2O3 / Y2O3 mixed slurry system, including a dispersant and a binder, and adopts a spray drying method to prepare composite granular particles in situ. Guided by the stability of the slurry, the amount of dispersant added is adjusted to change the combination state of Al2O3 and Y2O3, improve the mixing uniformity, and reduce the synthesis temperature of the YAG single phase. When the SHMP content is 1wt.%, the mixed slurry with a solid content of 45wt.% has the best stability after precipitation for 24 hours. Under this condition, the particles obtained by spray drying are monodisperse, dense and uniform spheres, and YAG single-phase particles are obtained by calcining at 1100°C in an air atmosphere. The method has simple process, low cost and energy consumption, high output, no environmental pollution, and is suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The SEM image and particle size distribution of the mixed spherical powder obtained in Example 1;

[0025] Figure 2 The SEM image and particle size distribution of the mixed spherical powder obtained in Example 2;

[0026] Figure 3 The scanning electron microscope image and particle size distribution of the mixed spherical powder obtained in Example 3;

[0027] Figure 4 The scanning electron microscope image and particle size distribution of the mixed spherical powder obtained in Example 4;

[0028] Figure 5 The scanning electron microscope image and particle size distribution of the mixed spherical powder obtained in Example 5;

[0029] Figure 6 The scanning electron microscope image and particle size distribution of the mixed spherical powder obtained in Comparative Example 1;

[0030] Figure 7 The XRD spectra of the mixed spherical powder obtained in Example 3 after calcination at different temperatures. DETAILED DESCRIPTION

[0031] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0032] In order to solve the technical problems of the prior art, the present invention provides a method for synthesizing spherical YAG powder in situ at low temperature by spray granulation technology, which can be carried out according to the following steps:

[0033] Mechanically stirring Y2O3 fine powder, Al2O3 powder, deionized water, dispersant, and binder to obtain a mixed slurry;

[0034] Y2O3 fine powder according to Y3Al5O 12 The stoichiometric ratio is mechanically stirred with Al2O3 powder and deionized water. After stirring for a certain period of time, a dispersant is added, and a binder is added before granulation to obtain a mixed slurry.

[0035] The solid content of the mixed slurry can be 30 to 60 wt.%;

[0036] The dispersant can be selected from one of ammonium citrate, sodium hexametaphosphate, polyvinyl butyral, and polyvinyl pyrrolidone, and the added amount is 0.1 to 2 wt.% of the powder mass;

[0037] The binder can be selected from one of polyvinyl alcohol and polyvinyl butyral, and the added amount is 0.1-1 wt.% of the powder mass.

[0038] The mixed slurry is sprayed and granulated to obtain spherical mixed powder;

[0039] The spray granulation method can be carried out by a spray dryer, the inlet temperature can be set to 150-300°C, the outlet temperature can be set to 50-200°C; the atomizer can be set to a speed of 30-50Hz;

[0040] D of the spherical mixed powder obtained by granulation 10 It can be 10 to 30 μm;

[0041] D of the spherical mixed powder obtained by granulation 50 It can be 10 to 100 μm;

[0042] D of the spherical mixed powder obtained by granulation 90 It can be 50 to 200 μm;

[0043] The fluidity index of the spherical mixed powder obtained by granulation is calculated by the Carr index method according to the Chinese national standard 31057.3-2018, which is the weighted sum of the repose angle, compression degree, flat angle, and uniformity index, and the value can be 70 to 90;

[0044] The repose angle of the spherical mixed powder obtained by granulation is the angle between the powder accumulation slope and the bottom horizontal plane in a static equilibrium state, which can be an acute angle and the angle can be 20 to 40°;

[0045] The compression degree of the spherical mixed powder obtained by granulation is the ratio of the difference between the tap density and the bulk density to the tap density, and the ratio can be 10 to 30%;

[0046] The plate angle of the spherical mixed powder obtained by granulation is the angle θ between the free surface (inclined surface) of the powder on the plate and the horizontal plane when the plate buried in the naturally accumulated powder is lifted vertically upward. S1 The angle θ after a certain impact S2 The average value of , the angle can be 30-50°;

[0047] The uniformity of the spherical mixed powder obtained by granulation is D 60 With D 10 The ratio can be 1 to 10.

[0048] The spherical mixed granulated powder is placed in a muffle furnace and calcined without pressure in an air atmosphere.

[0049] The air calcination condition may be a heating rate of 1 to 10°C / min;

[0050] The calcination temperature can range from 1000 to 1600°C;

[0051] The high temperature insulation time can be 2 to 10 hours.

[0052] Compared with the prior art, the advantages of the present invention include:

[0053] The Y2O3 micron powder provided can replace the expensive Y2O3 fine powder, and the production cost is low;

[0054] The spray granulation method provided enables the two powders to be dispersed evenly, and is simple to operate and has high production efficiency;

[0055] The calcination temperature of the in-situ synthesized spherical YAG provided is 300°C to 500°C lower than the synthesis temperature of the pure phase YAG synthesized by the traditional solid phase reaction method.

[0056] Next, several specific parameters are taken as examples to exemplify the specific implementation process of the present invention, and a comparative example is as follows:

[0057] Example 1

[0058] (1) According to Y3Al5O 12 According to the stoichiometric ratio, 150g of Al2O3 and 200g of refined Y2O3 were weighed respectively to prepare a slurry with a solid content of 60wt.%, and based on the total amount of all raw materials, 0.1wt.% of dispersant sodium hexametaphosphate, 1wt.% of binder polyvinyl alcohol, and deionized water were added and mechanically mixed to obtain a precursor slurry for spray granulation;

[0059] (2) The slurry obtained in step (1) was subjected to spray granulation at an inlet temperature of 260° C., an outlet temperature of 110° C., and an atomizer speed of 46 Hz to obtain 266 g of spherical mixed powder with a median particle size of 91.74 μm (eg Figure 1 As shown), the powder repose angle is 37°, the flat angle is 45°, the compression is 23.8%, the uniformity is 2.12, the fluidity index is 74.5, and the ratio of Y element to Al element is 0.44;

[0060] (3) The spherical mixed powder obtained in step (2) is calcined in air at 1400° C. for 4 h to obtain a pure YAG phase, thereby synthesizing spherical YAG powder in situ.

[0061] Example 2

[0062] (1) According to Y3Al5O 12 The stoichiometric ratio was 150 g of Al2O3 and 200 g of refined Y2O3 were weighed to prepare a slurry with a solid content of 30 wt.%. Based on the total amount of all raw materials, 2 wt.% of dispersant sodium hexametaphosphate, 0.1 wt.% of binder polyvinyl alcohol, and deionized water were added and mechanically mixed to obtain a precursor slurry for spray granulation. The other processes were the same as those in Example 1 to obtain a spherical mixed powder 273 (such as Figure 2 As shown), the powder repose angle is 36°, the flat angle is 47°, the compression is 19.7%, the uniformity is 1.85, the fluidity index is 78, and the ratio of Y element to Al element is 0.48;

[0063] (2) The spherical mixed powder obtained in step (1) is calcined in air at 1300° C. for 4 h to obtain a pure YAG phase, thereby synthesizing spherical YAG powder in situ.

[0064] Example 3

[0065] (1) According to Y3Al5O 12The stoichiometric ratio was 150 g of Al2O3 and 200 g of refined Y2O3 were weighed to prepare a slurry with a solid content of 45 wt.%. Based on the total amount of all raw materials, 1 wt.% of dispersant sodium hexametaphosphate, 0.5 wt.% of binder polyvinyl alcohol, and deionized water were added and mechanically mixed to obtain a precursor slurry for spray granulation. The other processes were the same as those in Example 1, and 285 g of spherical mixed powder with a median particle size of 38.57 μm (such as Figure 3 As shown), the powder repose angle is 30°, the flat angle is 43°, the compression degree is 15.9%, the uniformity is 2.16, the fluidity index is 83, and the ratio of Y element to Al element is 0.61;

[0066] (2) The spherical mixed powder obtained in step (1) is calcined in air at 1100° C. for 4 h to obtain a pure YAG phase, thereby synthesizing spherical YAG powder in situ.

[0067] Example 4

[0068] (1) According to Y3Al5O 12 The stoichiometric ratio was 150 g of Al2O3 and 200 g of refined Y2O3 were weighed to prepare a slurry with a solid content of 45 wt.%. Based on the total amount of all raw materials, 1 wt.% of dispersant polyvinyl butyral, 0.5 wt.% of binder polyvinyl alcohol, and deionized water were added and mechanically mixed to obtain a precursor slurry for spray granulation. The other processes were the same as those in Example 1, and 261 g of spherical mixed powder with a median particle size of 40.73 μm (such as Figure 4 As shown), the powder repose angle is 31°, the flat angle is 44°, the compression degree is 17%, the uniformity is 2.06, the fluidity index is 81, and the ratio of Y element to Al element is 0.67;

[0069] (2) The spherical mixed powder obtained in step (1) is calcined in air at 1400° C. for 4 h to obtain a pure YAG phase, thereby synthesizing spherical YAG powder in situ.

[0070] Example 5

[0071] (1) According to Y3Al5O 12 The stoichiometric ratio was 150 g of Al2O3 and 200 g of refined Y2O3 were weighed to prepare a slurry with a solid content of 45 wt.%. Based on the total amount of all raw materials, 1 wt.% of dispersant ammonium citrate, 0.5 wt.% of binder polyvinyl alcohol, and deionized water were added and mechanically mixed to obtain a precursor slurry for spray granulation. The other processes were the same as those in Example 1, and 292 g of spherical mixed powder with a median particle size of 37.86 μm (such as Figure 5As shown), the powder repose angle is 30°, the flat angle is 46°, the compression is 16.3%, the uniformity is 2.21, the fluidity index is 82, and the ratio of Y element to Al element is 0.52;

[0072] (2) The spherical mixed powder obtained in step (1) is calcined in air at 1500° C. for 4 h to obtain a pure YAG phase, thereby synthesizing spherical YAG powder in situ.

[0073] Comparative Example 1

[0074] (1) According to Y3Al5O 12 The stoichiometric ratio was 150 g of Al2O3 and 200 g of refined Y2O3 were weighed respectively to prepare a slurry with a solid content of 45 wt.%. Based on the total amount of all raw materials, no dispersant was added, 0.5 wt.% of binder polyvinyl alcohol and deionized water were added for mechanical mixing to obtain a precursor slurry for spray granulation. The other processes were the same as those in Example 1, and 274 g of spherical mixed powder with a median particle size of 42.74 μm was obtained (such as Figure 6 As shown), the powder repose angle is 32°, the flat angle is 47°, the compression is 17.2%, the uniformity is 2.18, the fluidity index is 78, and the ratio of Y element to Al element is 0.28;

[0075] (2) The spherical mixed powder obtained in step (1) is calcined in air at 1600° C. for 4 h to obtain a pure YAG phase, thereby synthesizing spherical YAG powder in situ.

[0076] Comparative Example 2

[0077] (1) According to Y3Al5O 12 According to the stoichiometric ratio, 150g of Al2O3 and 200g of refined Y2O3 were weighed respectively to prepare a slurry with a solid content of 45wt.%, and based on the total amount of all raw materials, 1wt.% of dispersant sodium hexametaphosphate was added and mechanically mixed with deionized water to obtain a precursor slurry;

[0078] (2) The slurry obtained in step (1) was placed in an oven at 80°C and dried, and passed through a 60-mesh sieve to obtain a mixed powder (such as Figure 7 As shown), the powder repose angle is 50°, the flat angle is 55°, the compression is 41.6%, the uniformity is 1.87, the fluidity index is 52.5, and the ratio of Y element to Al element is 0.23;

[0079] (3) The mixed powder obtained in step (2) is calcined in air at 1600° C. for 4 h to obtain a pure YAG phase.

[0080] Comparative Example 3

[0081] (1) According to Y3Al5O 12According to the stoichiometric ratio, 150g of Al2O3 and 200g of refined Y2O3 were weighed respectively to prepare a slurry with a solid content of 45wt.%;

[0082] (2) The slurry obtained in step (1) was placed in an oven at 80°C and dried, and passed through a 60-mesh sieve to obtain a mixed powder (such as Figure 7 As shown), the powder repose angle is 65°, the flat angle is 66°, the compression degree is 41.3%, the uniformity is 1.62, the fluidity index is 42, and the ratio of Y element to Al element is 0.11;

[0083] (3) The mixed powder obtained in step (2) is calcined in air at 1600° C. for 4 h to obtain a pure YAG phase.

[0084] Table 1

[0085]

[0086]

[0087] Table 2

[0088]

[0089] The Y2O3 / Al2O3 composite spherical powder prepared by the spray granulation process has a uniform particle size distribution. The particle size can be adjusted by changing the solid content and slurry viscosity, and it has the characteristics of high sphericity and high fluidity. The addition of dispersant can adjust the combination state of Al2O3 and Y2O3 and improve the mixing uniformity of the two. In the process of generating YAG phase by the high-temperature reaction of Al2O3 powder and Y2O3 powder, when the two powders are mixed evenly, the contact area between the components will increase, which helps to increase the effective contact between the reactants, making the diffusion and migration between Al2O3 and Y2O3 easier, thereby promoting the reaction and achieving the purpose of reducing the synthesis temperature of the YAG phase. When SHMP is used as a dispersant, the molar ratio of Y element to Al element in the granulated powder is 0.61, which is closest to the theoretical value. The YAG single phase is synthesized at a minimum of 1100°C, which is 300-500°C lower than the traditional YAG single phase synthesis temperature. In addition, the spray granulation method has a high production efficiency, and the powder produced can usually be produced on a large scale to meet the needs of industrial production.

Claims

1. A method for in-situ synthesis of spherical yttrium aluminum garnet powder by spray granulation technology, characterized in that: The steps include: S1, mechanically stirring yttrium oxide (Y2O3) powder, aluminum oxide (Al2O3) powder, deionized water, a dispersant, and a binder to obtain a mixed slurry; S2, spray granulating the mixed slurry to obtain spherical mixed powder; S3. placing the spherical mixed powder in a muffle furnace and calcining it without pressure in an air atmosphere.

2. The method according to claim 1, characterized in that The mixed slurry preparation comprises the following steps: S11, according to Y3Al5O 12 Yttrium oxide (Y2O3) powder, aluminum oxide (Al2O3) powder and deionized water are mechanically stirred and mixed in a stoichiometric ratio; S12, after stirring for a period of time, add dispersant and continue stirring; S13, adding a binder before granulation to obtain a mixed slurry.

3. The method according to claim 2, characterized in that In the step S11, the solid content of the mixed slurry is 30-60 wt.%.

4. The method according to claim 2, characterized in that In the step S12, the dispersant is selected from one of ammonium citrate, sodium hexametaphosphate, polyvinyl butyral, and polyvinyl pyrrolidone, and the added amount is 0.1-2 wt.% of the mass of the powder; The binder is selected from one of polyvinyl alcohol and polyvinyl butyral, and the added amount is 0.1-1wt.% of the powder mass.

5. The method according to claim 1, characterized in that In the step S2, the mixed slurry is granulated by a spray dryer, the inlet temperature of the spray dryer is 150-300°C, and the outlet temperature is 50-200°C; the atomizer speed of the spray dryer is 30-50Hz.

6. The method according to claim 1, characterized in that In the step S2, the particle size of the spherical mixed powder obtained by granulation is 10 to 100 μm.

7. The method according to claim 1, characterized in that In the step S2, the sphericity standard deviation of the spherical mixed powder obtained by granulation is 0 to 0.

3.

8. The method according to claim 1, characterized in that In the step S2, the fluidity index of the spherical mixed powder obtained by granulation is 70-90.

9. The method according to claim 1, characterized in that In step S3, the conditions of the calcination process are: a heating rate of 1 to 10°C / min; a calcination temperature range of 1000 to 1600°C; and a high temperature insulation time of 2 to 10 hours.

10. A spherical yttrium aluminum garnet (YAG), powder, characterized in that: The method is synthesized by any one of claims 1 to 9.

Citation Information

Patent Citations

  • Cerium-doped yttrium aluminum garnet transparent ceramic raw material and preparation method thereof

    CN114044668A

  • Method for preparing special-shaped YAG transparent ceramic through laser additive manufacturing technology

    CN116675535A

  • Yttrium aluminum garnet thermal barrier coating ceramic granulation powder as well as preparation method and application thereof

    CN117586001A

  • Production of yttrium-aluminum-garnet sintered compact and its starting material

    JP2001089225A

  • Method of producing transparent high-alloy er:YAG-ceramics

    RU2697561C1