3D printing zirconia composite ceramic slurry as well as preparation method and application thereof

By adding surface modifiers, dispersants, crosslinking agents and diluents to the 3D printed zirconia composite ceramic slurry, combined with 3D printing technology, the problems of different particle sizes and poor fluidity during the ceramic powder molding process are solved, and the problem of different particles and poor fluidity is achieved. The ceramic preparation with high solid content and low viscosity has been improved, and the hardness and mechanical properties of zirconia ceramics are suitable for the production of complex structures and spray drying equipment.

CN118908726APending Publication Date: 2024-11-08SHENZHEN MATERIAL TECH CO LTD

Patent Information

Application Number
CN202410952656.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

During the molding process of existing ceramic powder, there are problems such as different particle sizes, complex particle shapes and poor fluidity, which leads to uneven shrinkage and poor mechanical properties of ceramics after sintering, and severe wear and surface corrosion problems in spray drying technology. Influencing production continuity, photocuring 3D printing ceramic technology is difficult to take into account high solids content and low viscosity, resulting in a large performance gap.

Method used

Provide a 3D printed zirconia composite ceramic slurry containing ceramic powder, surface modifier, dispersant, crosslinking agent, diluent and photoinitiator to ensure high solids content and low viscosity through specific group distribution ratios and mixing methods. The slurry is prepared by 3D printing technology and has high hardness and excellent wear resistance, and is suitable for spray heads for spray drying.

Benefits of technology

It realizes the preparation of zirconia composite ceramic parts with high ceramic hardness, wear resistance and excellent mechanical properties. It is suitable for integrated molding of complex structures, improves the performance and production continuity of spray drying equipment, and reduces the viscosity to the final ceramic performance. Influence.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004947650620000141
    Figure BDA0004947650620000141
  • Figure BDA0004947650620000151
    Figure BDA0004947650620000151
Patent Text Reader

Abstract

The invention belongs to the technical field of ceramic materials, and particularly relates to 3D printing zirconia composite ceramic slurry as well as a preparation method and application thereof. The slurry comprises ceramic powder, a surface modifier, a dispersing agent, a cross-linking agent, a diluent and a photoinitiator, the mass of the surface modifier, the mass of the dispersant, the mass of the cross-linking agent, the mass of the diluent and the mass of the photoinitiator are respectively 8%-12%, 2%-6%, 12%-15%, 13%-16% and 3%-6% of the mass of the ceramic powder; the particle size of the ceramic powder is less than or equal to 10 microns; the ceramic powder comprises the following components in percentage by weight: 80%-94% of zirconium oxide, 1.5%-12% of yttrium oxide and 4.5%-15% of aluminum oxide. Due to the specific component proportion, the slurry can maintain low viscosity and support 3D printing forming while having high solid content, the performance of the finally obtained ceramic is not affected, and the obtained ceramic is excellent in mechanical property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of ceramic materials, and in particular relates to a 3D printing zirconia composite ceramic slurry and a preparation method and application thereof. Background Art

[0002] In the process of ceramic powder forming, the powder produced by manual powder making often has different particle sizes, complex particle shapes, poor fluidity, and uneven properties, which will eventually lead to uneven shrinkage of the sintered ceramics and local brittle fracture. The above defects can be avoided by using the spray drying method for ceramic powder forming. The method can be summarized as atomizing the thin material in a drying chamber, and then rapidly vaporizing the water in contact with hot air to obtain a dry product. This method can directly dry solutions and emulsions into powdery or granular products, eliminating the evaporation, crushing and other processes, and the resulting powder is small in size and basically spherical, which is convenient for counting the powder particle size. It can also meet the needs of ceramic powder pressure forming, has good fluidity, and the ceramic properties obtained after sintering are uniform.

[0003] In the existing spray drying technology, the spray head needs to rotate at high speed to throw out the mist droplets to contact the hot air for drying. However, due to the extremely high-speed rotation, the rotor of the spray head is seriously worn. If you are not careful during operation, the parts of the spray head may be separated, which will affect the continuity of the production process. At the same time, some ceramic slurries have a certain corrosive effect on the stainless steel surface coating of the spray head. There is a probability of corroding the stainless steel surface coating during the high temperature and high humidity spray process, so that the prepared powder is mixed with trace metal impurities.

[0004] As a new molding process with high printing speed, high precision and low cost, photocuring 3D printing technology can prepare various complex-shaped parts, bringing new manufacturing ideas for high-strength, high-hardness and difficult-to-process ceramic materials. However, there are still some problems with photocuring 3D printing ceramic technology. For example, photocuring ceramic slurry often cannot take into account both high solid content and low viscosity. During printing, layer-by-layer molding will easily lead to cracks and delamination, making the performance of the final product far different from that of ceramics molded by traditional processes, which is specifically manifested in poor mechanical properties. Summary of the invention

[0005] Therefore, the object of the present invention is to provide a 3D printed zirconia composite ceramic slurry and a preparation method and application thereof. The slurry can be used to prepare zirconia composite ceramic parts with high hardness, excellent wear resistance, various mechanical properties, and acid and alkali corrosion resistance using a 3D printing method, and can prepare complex parts by integral molding, and can be suitable for producing spray heads for spray drying with excellent production performance.

[0006] To this end, the present invention provides the following technical solutions.

[0007] The present invention provides a 3D printing zirconia composite ceramic slurry, comprising ceramic powder, a surface modifier, a dispersant, a cross-linking agent, a diluent, and a photoinitiator; the mass of the surface modifier is 8% to 12% of the ceramic powder; the mass of the dispersant is 2% to 6% of the ceramic powder; the mass of the cross-linking agent is 12% to 15% of the ceramic powder; the mass of the diluent is 13% to 16% of the ceramic powder; the mass of the photoinitiator is 3% to 6% of the ceramic powder; the particle size of the ceramic powder is ≤10μm; the ceramic powder contains the following components in weight percentage: 80% to 94% of zirconium oxide, 1.5% to 12% of yttrium oxide, and 4.5% to 15% of aluminum oxide.

[0008] Preferably, the ceramic powder contains 5.0% to 5.4% yttrium oxide.

[0009] Optionally, the surface modifier includes at least one of vinyl triethoxysilane, ammonium polyacrylate, polyoxyethylene sorbitan fatty acid ester, and sodium lignin sulfonate.

[0010] Optionally, the dispersant includes at least one of polyethylene glycol, triethylhexyl phosphoric acid, sodium pyrophosphate decahydrate, and polyether siloxane copolymer; wherein the molecular weight of the polyethylene glycol is 190 to 420, and the molecular weight of the polyether siloxane copolymer is 400 to 11,000.

[0011] Optionally, the cross-linking agent includes at least one of trimethylolpropane triacrylate, triallyl cyanurate, and tripropylene glycol diacrylate.

[0012] Optionally, the diluent includes at least one of hexanediol diacrylate, acryloyl morpholine, and isobornyl acrylate.

[0013] Optionally, the photoinitiator includes at least one of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, bis (4-tert-butylphenyl) iodonium hexafluorophosphate, and diethyl phosphite.

[0014] Preferably, the surface modifier is vinyltriethoxysilane.

[0015] Preferably, the crosslinking agent is trimethylolpropane triacrylate.

[0016] Preferably, the diluent is hexanediol diacrylate and acryloyl morpholine in a mass ratio of 4-6:6-4.

[0017] Preferably, the photoinitiator is diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide.

[0018] The present invention provides a method for preparing the above-mentioned 3D printing zirconia composite ceramic slurry, which comprises mixing the surface modifier, dispersant, cross-linking agent, diluent, photoinitiator and ceramic powder.

[0019] Preferably, the surface modifier, dispersant, cross-linking agent, diluent, and photoinitiator are mixed and slowly added into the ceramic powder under stirring, so as to achieve better mixing of the components and reduce the bonding of the ceramic powder.

[0020] Optionally, the stirring method includes mechanical stirring, ultrasonic oscillation stirring or magnetic stirring; preferably, the stirring method is ultrasonic oscillation stirring.

[0021] The present invention provides the use of the above-mentioned 3D printing zirconia composite ceramic slurry or the 3D printing zirconia composite ceramic slurry prepared by the above-mentioned preparation method in 3D printing to prepare zirconia composite ceramics.

[0022] Optionally, the 3D printing to prepare zirconia composite ceramics includes preparing an integrally formed zirconia composite ceramic part; preferably, the integrally formed zirconia composite ceramic part includes an integrally formed zirconia composite ceramic spray head.

[0023] Optionally, preparing zirconium oxide composite ceramics by 3D printing includes the following steps: 3D printing, removing support structures, and sintering.

[0024] In the application provided by the present invention, 3D printing molding, typically but not limitedly, includes the following steps: placing the slurry into the storage barrel of the light-curing 3D printer, converting the three-dimensional model image into a format and importing it into the printer, setting the layer thickness to 20 to 100 μm for printing.

[0025] In the application provided by the present invention, typically but not limitedly, a single extruder printer is used, and the material used for the support structure is the same as the composition of the printing slurry, which is a dendritic support structure automatically generated by the software on the surface of the part, and is used to assist the relative position of the part in the printing chamber to remain unchanged; when removing the support structure, first try to break it gently with your fingers, then slowly peel off the support structure, then rinse it with anhydrous ethanol, and finally spray the surface with a high-pressure air gun to dry the resulting blank.

[0026] Optionally, the sintering temperature curve is: a heating rate of 1 to 0.1°C / min, from room temperature to 200°C; a heating rate of 0.1 to 0.01°C / min, rising to 280°C, and keeping warm for 3 to 6 hours; a heating rate of 0.4 to 0.7°C / min, rising to 550°C, and keeping warm for 2 to 3 hours; a heating rate of 0.7 to 1°C / min, rising to 750°C; a heating rate of 1 to 2°C / min, rising to 900°C, and keeping warm for 1 hour; a heating rate of 0.1 to 0.5°C / min, rising to 1200°C, and keeping warm for 2 hours; a heating rate of 1 to 2.5°C / min, rising to the highest temperature, and keeping warm for 3 to 5 hours; a cooling rate of 1 to 1.5°C / min, from the highest temperature to 800°C; naturally cooling to room temperature; the highest temperature is 1480 to 1580°C; wherein the highest temperature is adaptively adjusted according to different furnace conditions.

[0027] Optionally, after the sintering step, a polishing step is also included; preferably, the polishing includes polishing using diamond particles; after the obtained ceramic is subjected to the diamond polishing process, the surface contact angle is large, the ceramic has good hydrophobic and oleophobic properties, is non-sticky, and is easy to clean.

[0028] The beneficial effects of the present invention are:

[0029] The 3D printing zirconium oxide composite ceramic slurry provided by the present invention comprises ceramic powder, a surface modifier, a dispersant, a cross-linking agent, a diluent, and a photoinitiator; the mass of the surface modifier is 8% to 12% of the ceramic powder; the mass of the dispersant is 2% to 6% of the ceramic powder; the mass of the cross-linking agent is 12% to 15% of the ceramic powder; the mass of the diluent is 13% to 16% of the ceramic powder; the mass of the photoinitiator is 3% to 6% of the ceramic powder; the particle size of the ceramic powder is ≤10μm; the ceramic powder contains the following components in weight percentage: 80% to 94% zirconium oxide, 1.5% to 12% yttrium oxide, and 4.5% to 15% aluminum oxide. The specific component ratio enables the slurry to maintain a low viscosity while having a high solid content and can support 3D printing, without affecting the performance of the final ceramic. The ceramic obtained has high hardness, excellent mechanical properties such as wear resistance, bending strength, compressive strength, and fracture toughness, low thermal expansion coefficient, and excellent impact resistance, and can adapt to high-speed rotation in high-temperature environments. In the ceramic powder, the role of yttrium oxide is to stabilize the grain structure during sintering, and the role of aluminum oxide is to enhance the toughness of zirconia ceramics.

[0030] The present invention provides the use of the above 3D printed zirconium oxide composite ceramic slurry or the 3D printed zirconium oxide composite ceramic slurry prepared by the above preparation method in 3D printing to prepare zirconium oxide composite ceramics; the 3D printing to prepare zirconium oxide composite ceramics includes preparing one-piece formed zirconium oxide composite ceramic parts. A preparation method for zirconium oxide ceramics having a relatively complex structure, which needs to be obtained by one-piece forming during preparation and has high requirements for mechanical properties, hardness and wear resistance is provided. DETAILED DESCRIPTION

[0031] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0032] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0033] Example 1

[0034] This embodiment provides a 3D printed zirconium oxide composite ceramic slurry and a preparation method thereof, comprising the following steps:

[0035] (1) 89.8% zirconium oxide, 5.2% yttrium oxide, and 5% aluminum oxide are taken and mixed to obtain ceramic powder, wherein the particle size of the ceramic powder is ≤10 μm.

[0036] (2) The surface modifier used is vinyl triethoxysilane, the dispersant is a polyether siloxane copolymer with a weight average molecular weight of 3000, the crosslinker is TMPTA (trimethylolpropane triacrylate), the diluent is a mixture of HDDA (hexanediol diacrylate) and ACMO (acryloyl morpholine) in a mass ratio of 4:5, and the photoinitiator is TPO (diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide). The surface modifier, dispersant, crosslinker, diluent, and photoinitiator are taken according to the mass of the ceramic powder, which is 10%, 3.5%, 14.8%, 13.2%, and 4.5%, respectively. The materials are mixed evenly and placed in an ultrasonic machine (Jiemeng JP-020S ultrasonic cleaning machine, ultrasonic power 120W, the same below), and the ceramic powder obtained in (1) is slowly added in an ultrasonic oscillation environment, mixed evenly, and a 3D printed zirconia composite ceramic slurry is obtained.

[0037] Example 2

[0038] This embodiment provides a 3D printed zirconium oxide composite ceramic slurry and a preparation method thereof, comprising the following steps:

[0039] (1) 91.2% zirconium oxide, 2.8% yttrium oxide, and 6% aluminum oxide are taken and mixed to obtain ceramic powder, wherein the particle size of the ceramic powder is ≤10 μm.

[0040] (2) The surface modifier used is vinyl triethoxysilane, the dispersant is a polyether siloxane copolymer with a weight average molecular weight of 6000, the crosslinker is TMPTA (trimethylolpropane triacrylate), the diluent is a mixture of HDDA (hexanediol diacrylate) and ACMO (acryloyl morpholine) in a mass ratio of 6:5, and the photoinitiator is TPO (diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide). The surface modifier, dispersant, crosslinker, diluent, and photoinitiator are taken according to the mass of the ceramic powder, which is 9%, 5%, 12.4%, 14.6%, and 3.8%, respectively. The materials are mixed evenly, placed in an ultrasonic machine, and the ceramic powder obtained in (1) is slowly added in an ultrasonic oscillation environment, mixed evenly, and a 3D printed zirconia composite ceramic slurry is obtained.

[0041] Example 3

[0042] This embodiment provides a 3D printed zirconium oxide composite ceramic slurry and a preparation method thereof, comprising the following steps:

[0043] (1) 80% zirconium oxide, 12% yttrium oxide, and 8% aluminum oxide are taken and mixed to obtain ceramic powder, wherein the particle size of the ceramic powder used is ≤10 μm.

[0044] (2) The surface modifier used is ammonium polyacrylate, the dispersant is triethylhexyl phosphate, the crosslinking agent is triallyl cyanurate, the diluent is a mixture of HDDA (hexanediol diacrylate) and ACMO (acryloyl morpholine) in a mass ratio of 4:6, and the photoinitiator is bis(4-tert-butylphenyl)iodonium hexafluorophosphate. The surface modifier, dispersant, crosslinking agent, diluent, and photoinitiator are taken according to the mass of the ceramic powder, which is 12%, 2%, 15%, 13%, and 6%, respectively. The materials are mixed evenly, placed in an ultrasonic machine, and the ceramic powder obtained in (1) is slowly added in an ultrasonic oscillation environment, mixed evenly, and a 3D printed zirconium oxide composite ceramic slurry is obtained.

[0045] Example 4

[0046] This embodiment provides a 3D printed zirconium oxide composite ceramic slurry and a preparation method thereof, comprising the following steps:

[0047] (1) 94% zirconium oxide, 1.5% yttrium oxide, and 4.5% aluminum oxide are taken and mixed to obtain ceramic powder, wherein the particle size of the ceramic powder used is ≤10 μm.

[0048] (2) The surface modifier used is polyoxyethylene sorbitan fatty acid ester, the dispersant is sodium pyrophosphate decahydrate, the crosslinker is tripropylene glycol diacrylate, the diluent is a mixture of HDDA (hexanediol diacrylate) and ACMO (acryloyl morpholine) in a mass ratio of 6:4, and the photoinitiator is diethyl phosphite. The surface modifier, dispersant, crosslinker, diluent, and photoinitiator are taken according to the mass of the ceramic powder, 8%, 6%, 12%, 16%, and 3%, respectively, mixed evenly, placed in an ultrasonic machine, and the ceramic powder obtained in (1) is slowly added in an ultrasonic oscillation environment, mixed evenly, and a 3D printed zirconia composite ceramic slurry is obtained.

[0049] Example 5

[0050] This embodiment provides a 3D printing zirconia composite ceramic slurry and a preparation method thereof, which is different from Embodiment 2 only in that, in step (1), yttrium oxide is 5.0% and aluminum oxide is 3.8%.

[0051] Example 6

[0052] This embodiment provides a 3D printing zirconia composite ceramic slurry and a preparation method thereof, which is different from Embodiment 2 only in that, in step (1), yttrium oxide is 5.4% and aluminum oxide is 3.4%.

[0053] Comparative Example 1

[0054] This comparative example provides a 3D printing zirconia composite ceramic slurry and a preparation method thereof, comprising the following steps:

[0055] (1) 70% zirconium oxide, 14% yttrium oxide, and 16% aluminum oxide are taken and mixed to obtain ceramic powder, wherein the particle size of the ceramic powder is ≤10 μm.

[0056] (2) The surface modifier used is ammonium polyacrylate, the dispersant is triethylhexyl phosphate, the crosslinking agent is triallyl cyanurate, the diluent is a mixture of HDDA (hexanediol diacrylate) and ACMO (acryloyl morpholine) in a mass ratio of 4:6, and the photoinitiator is bis(4-tert-butylphenyl)iodonium hexafluorophosphate. The surface modifier, dispersant, crosslinking agent, diluent, and photoinitiator are taken according to the mass of the ceramic powder, which is 6%, 15%, 10%, 10%, and 1%, respectively. The materials are mixed evenly, placed in an ultrasonic machine, and the ceramic powder obtained in (1) is slowly added in an ultrasonic oscillation environment, mixed evenly, and a 3D printed zirconium oxide composite ceramic slurry is obtained.

[0057] Comparative Example 2

[0058] This comparative example provides a 3D printing zirconia composite ceramic slurry and a preparation method thereof, comprising the following steps:

[0059] (1) Take 98% zirconium oxide, 1% yttrium oxide, and 1% aluminum oxide by mass, mix them to obtain ceramic powder, and the particle size of the ceramic powder used is ≤10 μm.

[0060] (2) The surface modifier used is ammonium polyacrylate, the dispersant is triethylhexyl phosphate, the crosslinking agent is triallyl cyanurate, the diluent is a mixture of HDDA (hexanediol diacrylate) and ACMO (acryloyl morpholine) in a mass ratio of 4:6, and the photoinitiator is bis(4-tert-butylphenyl)iodonium hexafluorophosphate. The surface modifier, dispersant, crosslinking agent, diluent, and photoinitiator are taken according to the mass of the ceramic powder, which is 16%, 1.2%, 17%, 10%, and 8%, respectively. The materials are mixed evenly, placed in an ultrasonic machine, and the ceramic powder obtained in (1) is slowly added in an ultrasonic oscillation environment, mixed evenly, and a 3D printed zirconium oxide composite ceramic slurry is obtained.

[0061] Embodiments 7 to 12

[0062] This embodiment provides an integrally formed zirconium oxide composite ceramic spray head prepared by 3D printing, comprising the following steps:

[0063] (1) Using a single extruder printer, take the slurries prepared in Examples 1 to 6 (corresponding to Examples 7 to 12 in order), place them in the storage barrel of the light-curing 3D printer, convert the three-dimensional model image into a format and import it into the printer, set the layer thickness to 25 μm for printing. During the printing process, the software automatically produces a tree-like support structure on the surface of the part. The material of the support structure is the same as the composition of the slurry involved in the printing. After printing is completed, slowly peel off the support structure, rinse it with anhydrous ethanol, and finally spray the surface with a high-pressure air gun to dry the resulting blank.

[0064] (2) After sintering and drying, the sintering temperature curve of the green body is as follows: the heating rate is 0.5℃ / min, from room temperature to 200℃; the heating rate is 0.05℃ / min, rising to 280℃, and keeping warm for 4h; the heating rate is 0.6℃ / min, rising to 550℃, and keeping warm for 2h; the heating rate is 0.7℃ / min, rising to 750℃; the heating rate is 1.5℃ / min, rising to 900℃, and keeping warm for 1h; the heating rate is 0.5℃ / min, rising to 1200℃, and keeping warm for 2h; the heating rate is 2℃ / min, rising to 1510℃, and keeping warm for 5h; the cooling rate is 1℃ / min, from 1510℃ to 800℃; and naturally cooling to room temperature.

[0065] (3) Fine machining: polishing with diamond particles to obtain a zirconium oxide composite ceramic spray head.

[0066] Embodiment 13

[0067] This embodiment provides an integrally formed zirconium oxide composite ceramic spray head prepared by 3D printing, comprising the following steps:

[0068] (1) Using a single extruder printer, take the slurry prepared in Example 2, place it in the storage barrel of a light-curing 3D printer, convert the three-dimensional model image into a format and import it into the printer, set the layer thickness to 50 μm for printing. During the printing process, the software automatically produces a tree-like support structure on the surface of the part, and the material of the support structure is the same as the slurry component involved in the printing. After printing is completed, slowly peel off the support structure, then rinse with anhydrous ethanol, and finally spray the surface with a high-pressure air gun to dry the resulting blank.

[0069] (2) After sintering and drying, the sintering temperature curve of the green body is as follows: the heating rate is 0.2℃ / min, from room temperature to 200℃; the heating rate is 0.04℃ / min, rising to 280℃, and keeping warm for 5h; the heating rate is 0.4℃ / min, rising to 550℃, and keeping warm for 2.5h; the heating rate is 0.8℃ / min, rising to 750℃; the heating rate is 1.7℃ / min, rising to 900℃, and keeping warm for 1h; the heating rate is 0.4℃ / min, rising to 1200℃, and keeping warm for 2h; the heating rate is 1.8℃ / min, rising to 1540℃, and keeping warm for 3h; the cooling rate is 1.2℃ / min, from 1540℃ to 800℃; and naturally cooling to room temperature.

[0070] (3) Fine machining: polishing with diamond particles to obtain a zirconium oxide composite ceramic spray head.

[0071] Embodiment 14

[0072] This embodiment provides an integrally formed zirconium oxide composite ceramic spray head prepared by 3D printing, comprising the following steps:

[0073] (1) Using a single extruder printer, take the slurry prepared in Example 2, place it in the storage barrel of a light-curing 3D printer, convert the three-dimensional model image into a format and import it into the printer, set the layer thickness to 50 μm for printing. During the printing process, the software automatically produces a tree-like support structure on the surface of the part, and the material of the support structure is the same as the slurry component involved in the printing. After printing is completed, slowly peel off the support structure, then rinse with anhydrous ethanol, and finally spray the surface with a high-pressure air gun to dry the resulting blank.

[0074] (2) After sintering and drying, the sintering temperature curve of the green body is as follows: the heating rate is 0.1℃ / min, from room temperature to 200℃; the heating rate is 0.01℃ / min, rising to 280℃, and keeping warm for 6h; the heating rate is 0.4℃ / min, rising to 550℃, and keeping warm for 3h; the heating rate is 0.7℃ / min, rising to 750℃; the heating rate is 1℃ / min, rising to 900℃, and keeping warm for 1h; the heating rate is 0.1℃ / min, rising to 1200℃, and keeping warm for 2h; the heating rate is 1℃ / min, rising to 1500℃, and keeping warm for 5h; the cooling rate is 1℃ / min, from 1500℃ to 800℃; and naturally cooling to room temperature.

[0075] (3) Fine machining: polishing with diamond particles to obtain a zirconium oxide composite ceramic spray head.

[0076] Embodiment 15

[0077] This embodiment provides an integrally formed zirconium oxide composite ceramic spray head prepared by 3D printing, comprising the following steps:

[0078] (1) Using a single extruder printer, take the slurry prepared in Example 2, place it in the storage barrel of a light-curing 3D printer, convert the three-dimensional model image into a format and import it into the printer, set the layer thickness to 50 μm for printing. During the printing process, the software automatically produces a tree-like support structure on the surface of the part, and the material of the support structure is the same as the slurry component involved in the printing. After printing is completed, slowly peel off the support structure, then rinse with anhydrous ethanol, and finally spray the surface with a high-pressure air gun to dry the resulting blank.

[0079] (2) After sintering and drying, the sintering temperature curve of the green body is as follows: the heating rate is 1℃ / min, from room temperature to 200℃; the heating rate is 0.1℃ / min, rising to 280℃, and keeping warm for 3h; the heating rate is 0.7℃ / min, rising to 550℃, and keeping warm for 2h; the heating rate is 1℃ / min, rising to 750℃; the heating rate is 2℃ / min, rising to 900℃, and keeping warm for 1h; the heating rate is 0.5℃ / min, rising to 1200℃, and keeping warm for 2h; the heating rate is 2.5℃ / min, rising to 1570℃, and keeping warm for 3h; the cooling rate is 1.5℃ / min, from 1570℃ to 800℃; and naturally cooling to room temperature.

[0080] (3) Fine machining: polishing with diamond particles to obtain a zirconium oxide composite ceramic spray head.

[0081] Comparative Examples 3 and 4

[0082] This comparative example provides an integrally formed zirconia composite ceramic spray head prepared by 3D printing, which differs from Example 7 only in that the 3D printed zirconia composite ceramic slurry prepared in Comparative Examples 1 and 2 (corresponding to Comparative Examples 3 and 4, respectively) are used in equal amounts to replace the 3D printed zirconia composite ceramic slurry prepared in Example 7. In the end, the zirconia composite ceramic spray head was not printed in both comparative examples.

[0083] Test Example 1

[0084] The ceramic slurries obtained in Examples 1 to 6 and Comparative Examples 1 and 2 were taken, and their solid content (refer to GB / T 1725-2007) and viscosity (refer to GB / T 17473.5-2008) were measured, and the obtained data are shown in Table 1. It can be seen from the data in Table 1 that compared with the ceramic slurries obtained in the examples, the ceramic slurries obtained in the comparative examples have similar solid contents, but too high viscosity and are not suitable for 3D printing.

[0085] Table 1

[0086] sample Solid content Viscosity (mPa·s) Example 1 40% 1950 Example 2 42% 1970 Example 3 30% 1050 Example 4 50% 3440 Example 5 41% 1940 Example 6 32% 1060 Comparative Example 1 44% 7043 Comparative Example 2 49% 8112

[0087] Test Example 2

[0088] Comparative Examples 3 and 4 failed to successfully print the zirconia composite ceramic spray head. Only the zirconia composite ceramic spray head obtained in Examples 7 to 15 was taken to test its density (using the drainage method, refer to GB / T2997-2015), hardness (reference GB / T16534-2009), and fracture toughness (reference 20220093-T-609). The results are shown in Table 2. The zirconia composite ceramic spray head prepared by 3D printing using the 3D printed zirconia composite ceramic slurry obtained in the embodiment of the present invention has high hardness and excellent fracture toughness, and can meet the use standard; while the ceramic slurry obtained in the comparative example cannot 3D print the target product, which is caused by the excessive viscosity and poor fluidity of the ceramic slurry obtained in Comparative Examples 1 and 2. Examples 8, 13, 14, and 15 all use the ceramic slurry obtained in Example 2. After the heating time is extended, the fracture toughness of Example 14 increases slightly and the hardness decreases slightly; after the sintering time is shortened, the density of Example 15 decreases slightly and the hardness increases slightly.

[0089] Table 2

[0090]

[0091]

[0092] Obviously, the above embodiments are merely examples for clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the protection scope of the invention.

Claims

1. A 3D printed zirconia composite ceramic slurry, characterized in that: Including ceramic powder, surface modifier, dispersant, cross-linking agent, diluent, photoinitiator; The mass of the surface modifier is 8% to 12% of the ceramic powder; The mass of the dispersant is 2% to 6% of the ceramic powder; The mass of the cross-linking agent is 12% to 15% of the ceramic powder; The mass of the diluent is 13% to 16% of the ceramic powder; The mass of the photoinitiator is 3% to 6% of the ceramic powder; The particle size of the ceramic powder is ≤10 μm; The ceramic powder contains the following components in weight percentage: 80% to 94% zirconium oxide, 1.5% to 12% yttrium oxide, and 4.5% to 15% aluminum oxide.

2. The 3D printing zirconia composite ceramic slurry according to claim 1, characterized in that: The ceramic powder contains 5.0% to 5.4% yttrium oxide.

3. The 3D printing zirconia composite ceramic slurry according to claim 1 or 2, characterized in that: The surface modifier includes at least one of vinyl triethoxysilane, ammonium polyacrylate, polyoxyethylene sorbitan fatty acid ester, and sodium lignin sulfonate; and / or, the dispersant comprises at least one of polyethylene glycol, triethylhexyl phosphoric acid, sodium pyrophosphate decahydrate, and polyether siloxane copolymer; And / or, the cross-linking agent includes at least one of trimethylolpropane triacrylate, triallyl cyanurate, and tripropylene glycol diacrylate; And / or, the diluent includes at least one of hexanediol diacrylate, acryloyl morpholine, and isobornyl acrylate; And / or, the photoinitiator includes at least one of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, bis (4-tert-butylphenyl) iodonium hexafluorophosphate, and diethyl phosphite.

4. The 3D printing zirconia composite ceramic slurry according to claim 3, characterized in that: The surface modifier is vinyl triethoxy silane; And / or, the cross-linking agent is trimethylolpropane triacrylate; and / or, the diluent is hexanediol diacrylate and acryloyl morpholine in a mass ratio of 4-6:6-4; And / or, the photoinitiator is diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide.

5. The method for preparing a 3D printed zirconia composite ceramic slurry according to any one of claims 1 to 4, characterized in that: The surface modifier, dispersant, cross-linking agent, diluent, photoinitiator and ceramic powder are mixed; preferably, the surface modifier, dispersant, cross-linking agent, diluent and photoinitiator are mixed and the ceramic powder is added under stirring.

6. Use of the 3D printing zirconia composite ceramic slurry according to any one of claims 1 to 4 or the 3D printing zirconia composite ceramic slurry prepared by the preparation method according to claim 5 in 3D printing to prepare zirconia composite ceramics.

7. The use according to claim 6, characterized in that: The 3D printing method for preparing zirconia composite ceramics includes preparing an integrally formed zirconia composite ceramic part; preferably, the integrally formed zirconia composite ceramic part includes an integrally formed zirconia composite ceramic spray head.

8. The use according to claim 6 or 7, characterized in that: 3D printing to prepare zirconia composite ceramics includes the following steps: 3D printing, removal of support structures, and sintering.

9. The use according to claim 8, characterized in that: The sintering temperature curve is as follows: the heating rate is 1-0.1°C / min, from room temperature to 200°C; the heating rate is 0.1-0.01°C / min, rising to 280°C, and keeping warm for 3-6h; the heating rate is 0.4-0.7°C / min, rising to 550°C, and keeping warm for 2-3h; the heating rate is 0.7-1°C / min, rising to 750°C; the heating rate is 1-2°C / min, rising to 900°C, and keeping warm for 1h; the heating rate is 0.1-0.5°C / min, rising to 1200°C, and keeping warm for 2h; the heating rate is 1-2.5°C / min, rising to the highest temperature, and keeping warm for 3-5h; the cooling rate is 1-1.5°C / min, from the highest temperature to 800°C; naturally cooling to room temperature; the highest temperature is 1480-1580°C.

10. The use according to claim 8 or 9, characterized in that: After the sintering step, a polishing step is also included; preferably, the polishing includes polishing with diamond particles.

Citation Information

Patent Citations

  • Ceramic slurry preparation and 3D (three dimensional) printing light curing molding method

    CN106810215A

  • Photocuring 3D printing alumina-based ceramic material as well as preparation method and application thereof

    CN115991595A

Cited By

  • Additive manufacturing method of yttrium oxide ceramic core

    CN119490352A