High-density boron nitride heat-conducting filler and preparation method thereof

Through the granulation and heat treatment method of hydrophilic modified hexagonal boron nitride and calcium acetate aqueous solution, the problems of low density and high preparation cost of hexagonal boron nitride ceramic materials were solved, and a high density boron nitride thermal filler was prepared, which significantly Improves the thermal conductivity of polymer composites.

CN118908737AActive Publication Date: 2024-11-08JIANGSU NOVORAY NEW MATERIAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411161568.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-08
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

In the prior art, the low density and high production cost of hexagonal boron nitride ceramic materials limit their application in high thermal conductivity fillers, especially in polymer composite materials with low filling amount, resulting in limited improvement in thermal conductivity.

Method used

By mixing the hydrophilic modified hexagonal boron nitride powder with calcium acetate aqueous solution, granulation and heat treatment, a high-density boron nitride thermal filler is formed, and calcium acetate is used to promote the slippage of boron nitride sheets and The sintered liquid phase is generated to increase its density and bond strength.

Benefits of technology

A high-density boron nitride thermal filler with a density of 1.9 to 2.0 g/cm3 was prepared at low cost and high yield, which significantly improved the thermal conductivity of polymer composites.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908737A_ABST
    Figure CN118908737A_ABST
Patent Text Reader

Abstract

The invention provides a high-density boron nitride heat-conducting filler and a preparation method thereof, and relates to the technical field of nitride ceramic materials. Hydrophilic modified hexagonal boron nitride is adopted, a calcium acetate aqueous solution is used as an auxiliary agent, the surface of boron nitride is hydrophilic, the boron nitride is wetted to generate lamellar slippage under the action of water in the auxiliary agent, meanwhile, calcium acetate has the effect similar to that of lubricating oil and also promotes lamellar slippage rearrangement of boron nitride, and high-density boron nitride particles are obtained through granulation; calcium acetate is decomposed to form calcium carbonate in the glue discharging process, calcium carbonate is further decomposed to form calcium oxide in the heat treatment process, the formed calcium oxide reacts with an oxidation film on the surface layer of boron nitride to generate a sintering liquid phase, meanwhile, growth of lamellar boron nitride grains is promoted, the bonding strength is improved, and then the high-density boron nitride heat conduction filler is obtained. When the polymer composite material is prepared, the polymer composite material has excellent heat-conducting property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nitride ceramic materials, and in particular to a high-density boron nitride thermal conductive filler and a preparation method thereof. Background Art

[0002] Hexagonal boron nitride is one of the key thermal conductive fillers to solve the heat dissipation problem of high-power electronic devices due to its excellent thermal conductivity, dielectric properties and chemical stability. In the preparation process of polymer composites, due to the significant thickening effect of the hexagonal boron nitride lamellar structure, its filling amount is low, which greatly limits the improvement of the thermal conductivity of the composite material. Spherical hexagonal boron nitride ceramic powder is an ideal filler for preparing polymer composites with high processability, high filling and high thermal conductivity. At present, spherical boron nitride thermal conductive fillers can be prepared by spray granulation, centrifugal granulation and other methods. Due to the strong covalent bond characteristics, hexagonal boron nitride is difficult to sinter without pressure. The spherical boron nitride prepared by the above method usually has a low density (<1.5g / cm 3 ). When preparing polymer composites by high shear dispersion, the spherical boron nitride powder is broken into lamellar powder again due to its low density and strength, causing the composite material to lose its processability.

[0003] The key to improving the filling performance of hexagonal nitrides is to increase their density. Currently, hot pressing and sintering methods can produce hexagonal nitrides with a density greater than 1.9 g / cm 3 Boron nitride ceramic materials. It has been reported that after crushing and screening the hot-pressed sintered boron nitride ceramics, the high-density boron nitride filler obtained can meet the high filling requirements of polymer composites. However, due to the limitations of hot-pressing sintering equipment, the preparation cost of hot-pressing sintering to prepare high-density boron nitride is high and the yield is low, which limits the application of this process in high thermal conductivity fillers. Therefore, a preparation method for high-density boron nitride with low preparation cost and yield is urgently needed. Summary of the invention

[0004] The purpose of the present invention is to provide a high-density boron nitride thermal conductive filler and a preparation method thereof. The preparation method provided by the present invention has low cost and high yield, and the prepared boron nitride thermal conductive filler has high density.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing a high-density boron nitride thermal conductive filler, comprising the following steps:

[0007] (1) mixing hydrophilic modified hexagonal boron nitride powder with a calcium acetate aqueous solution and granulating the mixture to obtain granulated powder;

[0008] (2) The granulated powder obtained in step (1) is subjected to debinding and heat treatment in sequence to obtain a high-density boron nitride thermal conductive filler.

[0009] Preferably, in the step (1), the average particle size of the hydrophilic modified hexagonal boron nitride powder is 5 to 30 μm, and the average sheet thickness of the hydrophilic modified hexagonal boron nitride powder is 0.5 to 2 μm.

[0010] Preferably, the mass concentration of the calcium acetate aqueous solution in step (1) is 5 to 15%.

[0011] Preferably, in step (1), the mass ratio of the hydrophilic modified hexagonal boron nitride powder to the calcium acetate aqueous solution is (10-20):1.

[0012] Preferably, the granulation pressure in step (1) is 200-300 MPa.

[0013] Preferably, the particle size of the granulated powder in step (1) is 50 to 500 μm.

[0014] Preferably, the debinding temperature in step (2) is 500-600° C., and the debinding time is 1-4 hours.

[0015] Preferably, the heat treatment temperature in step (2) is 1550-1650° C., and the heat treatment time is 1-6 hours.

[0016] The present invention also provides a high-density boron nitride thermal conductive filler prepared by the preparation method described in the above technical solution.

[0017] Preferably, the density of the high-density boron nitride thermal conductive filler is 1.9-2.0 g / cm 3 The tap density of high-density boron nitride thermal conductive filler is 0.9-1.1g / cm 3 .

[0018] The present invention provides a method for preparing a high-density boron nitride thermal conductive filler, comprising the following steps:

[0019] (1) mixing the hydrophilic modified hexagonal boron nitride powder with the calcium acetate aqueous solution and granulating to obtain granulated powder; (2) sequentially performing debinding and heat treatment on the granulated powder obtained in the step (1) to obtain a high-density boron nitride thermal conductive filler. The present invention adopts hydrophilic modified hexagonal boron nitride, and uses the calcium acetate aqueous solution as an auxiliary agent. The surface of the boron nitride is hydrophilic, and the wetting causes lamellar slip under the action of water in the auxiliary agent. At the same time, calcium acetate has a similar effect to lubricating oil, and also promotes the lamellar slip rearrangement of the boron nitride. After granulation, high-density boron nitride particles are obtained; during the debinding process, the calcium acetate decomposes to form calcium carbonate, and during the heat treatment process, the calcium carbonate further decomposes to form calcium oxide. The formed calcium oxide reacts with the oxide film on the surface of the boron nitride to generate a sintering liquid phase, and at the same time promotes the growth of lamellar boron nitride grains and improves the bonding strength, thereby obtaining a high-density boron nitride thermal conductive filler. When preparing a polymer composite material, the polymer composite material has excellent thermal conductivity. The preparation method provided by the present invention is not limited by high-pressure sintering equipment, and has low cost and high yield. The results of the examples show that the density of the boron nitride thermal conductive filler prepared by the present invention is 1.9-2.0 g / cm 3 , tap density is 0.9~1.1g / cm 3 . BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is the XRD pattern of the high-density boron nitride thermal conductive filler prepared in Example 1 of the present invention;

[0021] Figure 2 This is a SEM image of the high-density boron nitride thermal conductive filler prepared in Example 1 of the present invention;

[0022] Figure 3 This is a SEM image of the high-density boron nitride thermal conductive filler prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0023] The present invention provides a method for preparing a high-density boron nitride thermal conductive filler, comprising the following steps:

[0024] (1) mixing hydrophilic modified hexagonal boron nitride powder with a calcium acetate aqueous solution and granulating the mixture to obtain granulated powder;

[0025] (2) The granulated powder obtained in step (1) is subjected to debinding and heat treatment in sequence to obtain a high-density boron nitride thermal conductive filler.

[0026] Unless otherwise specified, the present invention has no particular limitation on the sources of the raw materials, and any commercially available product or product prepared by a conventional preparation method well known to those skilled in the art may be used.

[0027] The invention mixes hydrophilic modified hexagonal boron nitride powder with calcium acetate aqueous solution and then granulates to obtain granulated powder.

[0028] In the present invention, the average particle size of the hydrophilic modified hexagonal boron nitride powder is preferably 5 to 30 μm, more preferably 5 μm, 10 μm, 20 μm or 30 μm; the average sheet thickness of the hydrophilic modified hexagonal boron nitride powder is preferably 0.5 to 2 μm, more preferably 0.5 μm, 1 μm, 1.5 μm or 2 μm. The present invention limits the average particle size and average sheet thickness of the hydrophilic modified hexagonal boron nitride powder to the above range, which can further improve the density of boron nitride.

[0029] In the present invention, the water contact angle of the hydrophilic modified hexagonal boron nitride powder is preferably <90°. The present invention has no special limitation on the source of the hydrophilic modified hexagonal boron nitride powder. The product prepared by a commercial product or a conventional preparation method well known to those skilled in the art can be used as long as its water contact angle is <90°. In an embodiment of the present invention, the preparation method of the hydrophilic modified hexagonal boron nitride powder is preferably: thermally oxidizing the hexagonal boron nitride powder at 800°C for 4 hours in an air atmosphere to obtain the hydrophilic modified hexagonal boron nitride powder.

[0030] In the present invention, the mass concentration of the calcium acetate aqueous solution is preferably 5-15%, more preferably 5%, 10%, 12% or 15%. The present invention limits the mass concentration of the calcium acetate aqueous solution to the above range, which can further improve the density of boron nitride.

[0031] In the present invention, the mass ratio of the hydrophilic modified hexagonal boron nitride powder to the calcium acetate aqueous solution is preferably (10-20): 1, more preferably (14-20): 1, and further preferably (17-20): 1. The present invention limits the mass ratio of the hydrophilic modified hexagonal boron nitride powder to the calcium acetate aqueous solution within the above range, which can further improve the density of boron nitride.

[0032] The present invention has no special limitation on the mixing operation of the hydrophilic modified hexagonal boron nitride powder and the calcium acetate aqueous solution, and the two can be evenly mixed using a material mixing technical solution well known to those skilled in the art.

[0033] In the present invention, the granulation is preferably carried out in a dry roller granulator; the granulation pressure is preferably 200-300 MPa, more preferably 200-275 MPa, and further preferably 200-250 MPa. The present invention has no special limitation on the granulation time, as long as the particle size of the granulated powder is within the limited range. The present invention limits the granulation pressure within the above range, which can further improve the density of boron nitride.

[0034] After granulation, the present invention preferably sieves the granulated product to obtain granulated powder. The present invention has no special limitation on the sieving operation, and adopts the sieving technical scheme well known to those skilled in the art to ensure that the particle size of the granulated powder is within a limited range.

[0035] In the present invention, the particle size of the granulated powder is preferably 50-500 μm. The present invention limits the particle size of the granulated powder to the above range, which can ensure that the particle size of the prepared boron nitride is within this range, and can further improve the thermal conductivity of the composite material when used as a thermal conductive filler.

[0036] After obtaining the granulated powder, the present invention sequentially performs debinding and heat treatment on the granulated powder to obtain a high-density boron nitride thermal conductive filler.

[0037] In the present invention, the debinding temperature is preferably 500-600°C, more preferably 550-600°C; the debinding time is preferably 1-4h, more preferably 2-4h; the debinding is preferably carried out in an air atmosphere. In the present invention, during the debinding process, water in the calcium acetate aqueous solution evaporates, calcium acetate decomposes to form acetic acid and calcium carbonate, and acetic acid volatilizes. The present invention limits the debinding temperature and time within the above range, which can fully decompose calcium acetate and avoid oxidation of boron nitride.

[0038] In the present invention, the temperature of the heat treatment is preferably 1550-1650°C, more preferably 1600-1650°C; the time of the heat treatment is preferably 1-6h, more preferably 2-4h; the heat treatment is preferably carried out in a nitrogen atmosphere. In the present invention, during the heat treatment, calcium carbonate decomposes to form calcium oxide, and calcium oxide reacts with the oxide film on the surface of the boron nitride to generate a sintering liquid phase, which promotes the growth of lamellar boron nitride grains and improves the bonding strength to obtain a high-density boron nitride thermal conductive filler. The present invention limits the temperature and time of the heat treatment within the above range to further improve the density of the boron nitride.

[0039] After the heat treatment is completed, the present invention preferably cools the heat-treated product to obtain a high-density boron nitride thermally conductive filler.

[0040] The present invention has no special limitation on the cooling operation, and cooling to room temperature may be performed using cooling technical solutions well known to those skilled in the art.

[0041] The invention adopts hydrophilic modified hexagonal boron nitride and uses calcium acetate aqueous solution as an auxiliary agent. The surface of the boron nitride is hydrophilic, and the boron nitride is wetted to cause lamellar slip under the action of water in the auxiliary agent. Meanwhile, calcium acetate has a function similar to lubricating oil and also promotes lamellar slip rearrangement of the boron nitride. After granulation, high-density boron nitride particles are obtained. During the debinding process, the calcium acetate is decomposed to form calcium carbonate. During the heat treatment process, the calcium carbonate is further decomposed to form calcium oxide. The formed calcium oxide reacts with an oxide film on the surface of the boron nitride to generate a sintering liquid phase, and at the same time, the growth of lamellar boron nitride grains is promoted and the bonding strength is improved. The process parameters such as the amount of each raw material, the reaction temperature, etc. are controlled to obtain a high-density boron nitride thermal conductive filler. When the polymer composite material is prepared, the polymer composite material has excellent thermal conductivity.

[0042] The present invention also provides a high-density boron nitride thermal conductive filler prepared by the preparation method described in the above technical solution.

[0043] In the present invention, the density of the high-density boron nitride thermal conductive filler is preferably 1.9 to 2.0 g / cm 3 The tap density of the high-density boron nitride thermal conductive filler is preferably 0.9 to 1.1 g / cm 3 .

[0044] The boron nitride thermal conductive filler prepared by the invention has high density, and when the polymer composite material is prepared, the polymer composite material has excellent thermal conductive performance.

[0045] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0046] The preparation method of the hydrophilic modified hexagonal boron nitride powder in each embodiment is: thermally oxidizing the hexagonal boron nitride powder at 800° C. for 4 hours in an air atmosphere to obtain the hydrophilic modified hexagonal boron nitride powder.

[0047] Example 1

[0048] (1) mixing surface hydrophilic modified hexagonal boron nitride powder with an average particle size of 5.0 μm and an average lamella thickness of 0.5 μm with a calcium acetate aqueous solution with a mass concentration of 15% (the mass ratio of surface hydrophilic modified hexagonal boron nitride powder to calcium acetate aqueous solution is 10:1), granulating with a dry roller granulator at a pressure of 300 MPa, and sieving to obtain granulated powder with a particle size of 50 to 500 μm;

[0049] (2) The granulated powder obtained in step (1) is subjected to debinding at 600° C. in an air atmosphere for 4 h, and then heat-treated at 1550° C. in a nitrogen atmosphere for 4 h, and cooled to obtain a high-density boron nitride thermal conductive filler.

[0050] The particle size of the high-density boron nitride thermal conductive filler prepared in Example 1 was measured to be in the range of 50 to 500 μm, and the density was 1.90 g / cm 3 , tap density is 0.90g / cm 3 .

[0051] The high-density boron nitride thermal conductive filler prepared in Example 1 was subjected to XRD testing, and the obtained XRD pattern is as follows: Figure 1 As shown. Figure 1 It can be seen that the phase composition of the high-density boron nitride thermal conductive filler is h-BN, without impurity phase; on the one hand, it may be because the impurity phase volatilizes at high temperature during the heat treatment process, and on the other hand, it may be because the impurity phase content is too small to be detected.

[0052] The high-density boron nitride thermal conductive filler prepared in Example 1 was observed using a scanning electron microscope, and the obtained SEM image is as follows: Figure 2 As shown. Figure 2 It can be seen that the prepared high-density boron nitride thermal conductive filler is composed of oriented and closely stacked BN sheets.

[0053] Example 2

[0054] (1) mixing a surface hydrophilic modified hexagonal boron nitride powder having an average particle size of 10.0 μm and an average lamella thickness of 1.0 μm with a calcium acetate aqueous solution having a mass concentration of 12% (the mass ratio of the surface hydrophilic modified hexagonal boron nitride powder to the calcium acetate aqueous solution is 14:1), granulating the mixture with a dry roller granulator at a pressure of 275 MPa, and obtaining a granulated powder having a particle size of 50 to 500 μm after sieving;

[0055] (2) The granulated powder obtained in step (1) is subjected to debinding at 600° C. in an air atmosphere for 4 h, and then heat-treated at 1600° C. in a nitrogen atmosphere for 4 h, and cooled to obtain a high-density boron nitride thermal conductive filler.

[0056] The particle size of the high-density boron nitride thermal conductive filler prepared in Example 2 was measured to be in the range of 50 to 500 μm, and the density was 1.93 g / cm 3 , tap density is 0.97g / cm 3 .

[0057] The high-density boron nitride thermal conductive filler prepared in Example 2 was subjected to XRD test, and its phase composition was h-BN without any impurity phase.

[0058] The high-density boron nitride thermal conductive filler prepared in Example 2 was observed using a scanning electron microscope, and the obtained SEM image is as follows: Figure 3 As shown. Figure 3 It can be seen that the prepared high-density boron nitride thermal conductive filler is composed of oriented and closely stacked BN sheets.

[0059] Example 3

[0060] (1) mixing surface hydrophilic modified hexagonal boron nitride powder with an average particle size of 20.0 μm and an average lamella thickness of 1.5 μm with a calcium acetate aqueous solution with a mass concentration of 10% (the mass ratio of surface hydrophilic modified hexagonal boron nitride powder to calcium acetate aqueous solution is 17:1), granulating with a dry roller granulator at a pressure of 250 MPa, and sieving to obtain granulated powder with a particle size of 50 to 500 μm;

[0061] (2) The granulated powder obtained in step (1) is subjected to debinding at 600° C. in an air atmosphere for 4 h, and then heat-treated at 1600° C. in a nitrogen atmosphere for 4 h, and cooled to obtain a high-density boron nitride thermal conductive filler.

[0062] The particle size of the high-density boron nitride thermal conductive filler prepared in Example 3 was measured to be in the range of 50 to 500 μm, and the density was 1.96 g / cm 3 , tap density is 1.03g / cm 3 .

[0063] The high-density boron nitride thermal conductive filler prepared in Example 3 was subjected to XRD test, and its phase composition was h-BN without any impurity phase.

[0064] The high-density boron nitride thermal conductive filler prepared in Example 3 was observed using a scanning electron microscope. The prepared high-density boron nitride thermal conductive filler was formed by closely stacked oriented BN sheets.

[0065] Example 4

[0066] (1) mixing a surface hydrophilic modified hexagonal boron nitride powder having an average particle size of 30.0 μm and an average lamella thickness of 2.0 μm with a calcium acetate aqueous solution having a mass concentration of 5% (the mass ratio of the surface hydrophilic modified hexagonal boron nitride powder to the calcium acetate aqueous solution is 20:1), granulating the mixture by a dry roller granulator at a pressure of 200 MPa, and obtaining a granulated powder having a particle size of 50 to 500 μm by sieving;

[0067] (2) The granulated powder obtained in step (1) is subjected to debinding at 600° C. in an air atmosphere for 4 h, and then heat-treated at 1650° C. in a nitrogen atmosphere for 4 h, and cooled to obtain a high-density boron nitride thermal conductive filler.

[0068] The particle size of the high-density boron nitride thermal conductive filler prepared in Example 4 was measured to be in the range of 50 to 500 μm and the density was 2.0 g / cm 3 , tap density is 1.10g / cm 3 .

[0069] The high-density boron nitride thermal conductive filler prepared in Example 4 was subjected to XRD test, and its phase composition was h-BN without any impurity phase.

[0070] The high-density boron nitride thermal conductive filler prepared in Example 4 was observed using a scanning electron microscope. The prepared high-density boron nitride thermal conductive filler was formed by closely stacked oriented BN sheets.

[0071] Examples 5 to 8, Comparative Examples 1 to 9

[0072] The average particle size of the surface hydrophilic modified hexagonal boron nitride powder (h-BN), the mass ratio of the surface modified hexagonal boron nitride powder to the calcium acetate aqueous solution, and the concentration of the calcium acetate aqueous solution in Example 1 were changed according to Table 1 to prepare boron nitride. The density and tap density of the obtained boron nitride are shown in Table 1.

[0073] Table 1 Average particle size of surface hydrophilic modified hexagonal boron nitride powder, mass ratio of surface modified hexagonal boron nitride powder to calcium acetate aqueous solution, concentration of calcium acetate aqueous solution, density and tap density of prepared boron nitride in Examples 5 to 8 and Comparative Examples 1 to 9

[0074]

[0075]

[0076] It can be seen from Table 1 that when the average particle size of the surface hydrophilic modified hexagonal boron nitride powder is less than 5 μm and greater than 30 μm, the density and tap density of the obtained boron nitride are reduced; when the mass ratio of the surface hydrophilic modified hexagonal boron nitride powder to the calcium acetate aqueous solution is higher than 10:1 or lower than 20:1, the density and tap density of the obtained boron nitride are reduced; when the concentration of calcium acetate is less than 5wt% or greater than 15%, the density and tap density of the obtained boron nitride are reduced, and when it is higher than 15%, the generation of impurities is detected.

[0077] Examples 9 to 12, Comparative Examples 10 to 13

[0078] The granulation pressure and the heat treatment temperature in Example 2 were changed according to Table 2 to prepare boron nitride. The density and tap density of the prepared boron nitride are shown in Table 2.

[0079] Table 2 Granulation pressure, heat treatment temperature, density and tap density of the prepared boron nitride in Examples 9 to 12 and Comparative Examples 10 to 13

[0080] Pressure(MPa) Heat treatment temperature(℃) <![CDATA[Density (g / cm 3 )]]> <![CDATA[Tap density (g / cm 3 )]]> Example 9 200 1600 1.91 0.90 Example 10 250 1600 1.93 0.94 Embodiment 11 300 1600 1.95 1.01 Example 12 275 1650 1.92 0.94 Comparative Example 10 175 1600 1.81 0.79 Comparative Example 11 325 1600 1.95 1.01 Comparative Example 12 275 1500 1.89 0.88 Comparative Example 13 275 1700 1.87 0.86

[0081] It can be seen from Table 2 that when the granulation roller pressure is less than 200MPa, the density and tap density of the obtained boron nitride are reduced, while when it is greater than 300MPa, the density and tap density do not increase significantly; when the sintering temperature is lower than 1550℃ or higher than 1650℃, the density and tap density of the obtained boron nitride are reduced.

[0082] Application Examples

[0083] The high-density boron nitride prepared in Examples 1 to 4 was stirred and mixed with bisphenol A type E51 epoxy resin under vacuum conditions, the mass ratio of boron nitride to bisphenol A type E51 epoxy resin was 50:50 (the mass content of boron nitride in the polymer composite material was 50%), and the polymer composite material was cured at 160° C. for 4 hours to obtain a polymer composite material.

[0084] The thermal conductivity of the prepared polymer composite material was measured using a flat plate thermal conductivity method, and the results are shown in Table 3.

[0085] Table 3 Thermal conductivity of polymer composites prepared from high density boron nitride prepared in Examples 1 to 4

[0086] Thermal conductivity (W / (m·K)) Example 1 1.81 Example 2 1.87 Example 3 1.92 Example 4 1.98

[0087] It can be seen from Table 3 that the filling amount of the high-density boron nitride thermal conductive filler prepared in the present invention in the polymer composite material is relatively high, and the prepared polymer composite material has excellent thermal conductivity.

[0088] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a high-density boron nitride thermal conductive filler, comprising the following steps: (1) mixing hydrophilic modified hexagonal boron nitride powder with a calcium acetate aqueous solution and granulating the mixture to obtain granulated powder; (2) The granulated powder obtained in step (1) is subjected to debinding and heat treatment in sequence to obtain a high-density boron nitride thermal conductive filler.

2. The preparation method according to claim 1, characterized in that: In the step (1), the average particle size of the hydrophilic modified hexagonal boron nitride powder is 5 to 30 μm, and the average sheet thickness of the hydrophilic modified hexagonal boron nitride powder is 0.5 to 2 μm.

3. The preparation method according to claim 1, characterized in that: The mass concentration of the calcium acetate aqueous solution in step (1) is 5-15%.

4. The preparation method according to claim 3, characterized in that: In the step (1), the mass ratio of the hydrophilic modified hexagonal boron nitride powder to the calcium acetate aqueous solution is (10-20):

1.

5. The preparation method according to claim 1, characterized in that: The granulation pressure in the step (1) is 200-300 MPa.

6. The preparation method according to claim 1, characterized in that: The particle size of the granulated powder in step (1) is 50 to 500 μm.

7. The preparation method according to claim 1, characterized in that: In the step (2), the debinding temperature is 500-600° C., and the debinding time is 1-4 hours.

8. The preparation method according to claim 1, characterized in that: The heat treatment temperature in step (2) is 1550-1650° C., and the heat treatment time is 1-6 hours.

9. The high-density boron nitride thermal conductive filler prepared by the preparation method according to any one of claims 1 to 8.

10. The high-density boron nitride thermally conductive filler according to claim 9, characterized in that: The density of the high-density boron nitride thermal conductive filler is 1.9-2.0 g / cm 3 The tap density of high-density boron nitride thermal conductive filler is 0.9-1.1g / cm 3 .

Citation Information

Patent Citations

  • Preparation method of spherical hexagonal boron nitride aggregate

    CN108101546A

  • Preparation method of magnesium oxide and boron nitride composite microspheres

    CN113735569A

  • Spherical hexagonal boron nitride and preparation method thereof

    CN115974011A

  • Preparation and strength characterization method of spherical boron nitride with high density and controllable granularity

    CN116693299A

  • Hexagonal boron nitride material as well as preparation method and application thereof

    CN117800739A