Energy-saving light-weight castable for mouth of cement kiln and preparation method of energy-saving light-weight castable
By reasonably preparing lightweight lanthanum aluminate-mullite aggregate and other components in cement kiln materials, the porosity and infrared emission capacity are improved, and the problem of insufficient insulation performance of cement kiln materials is solved, and the problem of the cement kiln material is achieved High efficiency, energy saving and fire resistance.
Patent Information
- Application Number
- CN202411252187.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-09
AI Technical Summary
The thermal insulation performance of existing cement kiln kiln materials cannot meet the energy-saving needs of the cement industry. Infrared radiation materials have limited role in heat transfer in high-temperature environments, and refractory materials are prone to damage during service, resulting in short service life.
60 to 70 parts of lightweight lanthanum aluminate-mullite aggregate, 5 to 10 parts of silicon carbide fine powder, 8 to 12 parts of alumina fine powder, 4 to 8 parts of plate-shaped corundum fine powder, 1 ~3 parts of α-Al2O3 fine powder, 1 to 6 parts of lanthanum zirconate fine powder, 4 to 6 parts of calcium aluminate cement and 0.1 to 0.2 parts of water reducing agent, energy-saving lightweight cement kiln is prepared by ball milling and calcining. Kiln castable material improves the porosity and infrared emission capability of the material.
Significantly reduce heat transfer in kiln lining, improve the thermal radiation reflection ability of the material, enhance fire resistance and toughness, extend service life, reduce heat loss, achieve low thermal conductivity and high infrared emissivity, and significantly reduce energy consumption in the cement kiln kiln area .
Smart Images

Figure CN118908740A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of refractory materials, and in particular relates to an energy-saving lightweight cement kiln mouth castable and a preparation method thereof. Background Art
[0002] my country's cement industry is a typical high-energy consumption industry. The service temperature of the cement kiln body is between 1100 and 1500℃, which is the hottest part in the cement production system. The current cement kiln mouth generally uses mullite silicon carbide castable as the lining material, which is the area with the most severe service environment and heat dissipation. Therefore, the energy saving and heat preservation of the cement kiln mouth is of great significance to the key energy and emission reduction of the cement industry. In order to improve the thermal insulation performance of the kiln body, cement kilns have begun to use lightweight refractory materials as kiln linings in recent years. In order to ensure the wear resistance and strength of the kiln lining refractory materials, the improvement of the porosity in lightweight refractory materials is relatively limited compared with the dense kiln lining refractory materials, and the energy saving and heat preservation effect on the kiln lining is also relatively limited. In order to further improve the thermal insulation performance of the cement kiln mouth, it is urgent to develop an energy-saving castable that can meet the service of the cement kiln mouth and meet the current needs of cement energy saving and emission reduction.
[0003] In recent years, infrared radiation materials have been widely used as energy-saving materials for high-temperature linings. This material can achieve the purpose of energy saving and heat preservation to a certain extent due to its high infrared emission ability. However, the transfer of heat in the kiln lining at high temperatures is still mainly heat conduction, and thermal radiation still occupies a relatively small part in heat transfer. Therefore, the energy-saving and heat-insulating effect of infrared radiation materials on kiln linings is still relatively limited. At present, there is still a lack of reports on combining the characteristics of infrared radiation materials with the porous structure of kiln linings to improve the thermal insulation performance of kiln lining refractory materials.
[0004] CN202410022481.X discloses an environmentally friendly chromium-containing spinel infrared radiation coating, which uses aluminum-chromium solid solution fine powder, zirconium oxide fine powder and silica sol as transition layer raw materials, and titanium-iron co-doped magnesium-chromium spinel fine powder, aluminum-chromium solid solution fine powder, boron-containing glass powder, silicon micropowder and aluminum dihydrogen phosphate solution as working layer raw materials. Applying it on the surface of the lining can effectively improve the thermal efficiency of the kiln body. However, this infrared radiation coating is severely worn with coal powder and cement raw materials during the service of cement kilns, which easily leads to mechanical peeling and failure of the coating structure.
[0005] CN202310563163.X discloses a lightweight high thermal shock refractory material for cement kiln preheating decomposition zone and a preparation method thereof. The lightweight high thermal shock refractory material is mainly composed of raw materials such as coke, silicon carbide, andalusite, α-Al2O3 powder, kaolinite and bonding clay. However, lightweight refractory materials only reduce the thermal conductivity efficiency of the material by increasing the porosity, and do not comprehensively consider the influence of high-temperature thermal radiation on heat dissipation. Therefore, its energy-saving effect on the kiln body is relatively limited.
[0006] The problem that the thermal insulation performance of existing cement kiln lining materials cannot meet the energy-saving needs of cement kilns; the energy saving of cement kiln bodies can be further achieved by synergizing the components and structure of refractory materials to achieve thermal insulation and high infrared emission capabilities. Summary of the invention
[0007] In view of the shortcomings of the prior art, the present invention provides an energy-saving lightweight cement kiln mouth castable and a preparation method thereof. The castable prepared by the present invention can significantly reduce the heat transfer in the kiln lining while improving the reflection ability of infrared radiation. The product has the advantages of high strength, good thermal shock stability, excellent thermal insulation performance, high thermal radiation absorption rate and emission efficiency, low cost, simple preparation process, etc. It can significantly increase the service life of the kiln mouth refractory material while reducing heat loss, and has good application prospects.
[0008] To achieve the above objectives, the present invention adopts the following technical solutions.
[0009] An energy-saving lightweight cement kiln mouth castable comprises the following components in parts by mass: 60-70 parts of lightweight lanthanum aluminate-mullite aggregate, 5-10 parts of silicon carbide fine powder, 8-12 parts of alumina fine powder, 4-8 parts of plate-shaped corundum fine powder, 1-3 parts of α-Al2O3 micropowder, 1-6 parts of lanthanum zirconate fine powder, 4-6 parts of calcium aluminate cement, 0.1-0.2 parts of water reducer and 5-6 parts of water.
[0010] Furthermore, the particle gradation of the lightweight lanthanum aluminate-mullite aggregate is: the particle size of 3-5 mm accounts for 40-50wt% of the lightweight lanthanum aluminate-mullite aggregate, the particle size of 1-3 mm accounts for 25-40wt% of the lightweight lanthanum aluminate-mullite aggregate, and the particle size of 0.1-1 mm accounts for 10-25wt% of the lightweight lanthanum aluminate-mullite aggregate; the porosity of the lightweight lanthanum aluminate-mullite aggregate is ≥50%, the average pore size is 2-20 μm, and the lanthanum aluminate content is ≥50wt%.
[0011] Furthermore, the particle size of the silicon carbide fine powder is ≤0.088 mm, and the SiC content of the silicon carbide fine powder is ≥90 wt%.
[0012] Furthermore, the particle size of the alumina fine powder is ≤0.088 mm, and the Al2O3 content in the alumina fine powder is ≥60 wt%.
[0013] Furthermore, the particle size of the plate-like corundum fine powder is ≤0.088 mm, and the Al2O3 content in the plate-like corundum fine powder is ≥99wt%.
[0014] Furthermore, the particle size of the α-Al2O3 micropowder is ≤2μm, and the Al2O3 content in the α-Al2O3 micropowder is ≥98wt%.
[0015] Furthermore, the particle size of the lanthanum zirconate fine powder is ≤ 88 μm, and the La2Zr2O7 content in the lanthanum zirconate fine powder is ≥ 99 wt%.
[0016] Furthermore, the Al2O3 content in the calcium aluminate cement is ≥71wt%.
[0017] Furthermore, the water reducing agent is one of sodium tripolyphosphate, sodium hexametaphosphate, FS10 or FS20.
[0018] A method for preparing an energy-saving lightweight cement kiln mouth castable comprises the following steps: Step 1, 4 to 12 parts of mullite fine powder, 1 to 3 parts of mullite micropowder, 2 to 6 parts of lanthanum aluminate fine powder, and 4 to 12 parts of dextrin are mixed, and ball-milled for 4 to 8 hours to obtain ball-milled powder; 6 to 10 parts of water are added to the ball-milled powder, granulated to obtain prefabricated spherical aggregates of different particle sizes, and dried at 110° C. for 24 to 36 hours; and the dried spherical aggregates are calcined under certain conditions, sieved, and lightweight lanthanum aluminate-mullite aggregates are obtained.
[0019] Step 2: first use 60-70 parts of lightweight lanthanum aluminate-mullite aggregate, 5-10 parts of silicon carbide fine powder, 8-12 parts of alumina fine powder, 4-8 parts of plate-shaped corundum fine powder, 1-3 parts of α-Al2O3 micropowder, 1-6 parts of lanthanum zirconate fine powder, and 4-6 parts of calcium aluminate cement as raw materials, add 0.1-0.2 parts of water reducer to the raw materials, mix well, then add 5-6 parts of water to the raw materials, stir well, shape, cure for 2-3 days, demold, and bake to obtain energy-saving lightweight cement kiln mouth castable.
[0020] Furthermore, in the step 1, the Al2O3 content in the mullite fine powder is ≤70wt%; the Al2O3 content in the mullite micropowder is ≤70wt%.
[0021] Furthermore, in step 1, the particle size of the prefabricated spherical aggregate is 5-3 mm, 3-1 mm and 1-0 mm.
[0022] Furthermore, in step 1, the calcination temperature is 1200-1400° C., and the calcination time is 3-8 hours.
[0023] Compared with the prior art, the beneficial effects of the present invention are as follows.
[0024] 1. First, the pouring construction method involved in the present invention avoids the high-temperature firing process, which is beneficial to energy conservation and environmental protection. Secondly, the aggregate part in the refractory material accounts for 60-70% of the total weight. The introduction of lightweight lanthanum aluminate-mullite aggregate not only ensures the overall lightweight and porosity of the kiln mouth refractory material, while ensuring the overall strength and wear resistance, but also improves the internal thermal resistance of the material by increasing the porosity, blocking the conduction of heat, and improves the infrared emission and reflection ability of the material at high temperature through the high emissivity of the aggregate itself, reduces radiation heat dissipation, and increases energy utilization; under the same preparation conditions, the thermal conductivity and average emissivity of the lightweight kiln mouth castable prepared by the present invention are better than other materials.
[0025] 2. Introduce lanthanum zirconate fine powder into the refractory matrix. The addition of lanthanum zirconate fine powder can improve the toughness of the refractory material and optimize and improve its thermal shock stability. In addition, lanthanum zirconate itself has a high infrared emissivity, which can also synergistically improve its ability to reflect radiation.
[0026] 3. At present, infrared radiation materials are often directly coated on the surface of refractory materials in the form of coatings. In cement kilns, the coatings are very easy to peel off due to the intense friction between the kiln lining and cement. Therefore, the infrared radiation components are directly introduced into the refractory components, and their infrared radiation characteristics will be retained under complex service conditions. The present invention prepares the main component of the refractory material, the aggregate, into a lightweight aggregate with infrared emission capabilities, and the lanthanum zirconate in the matrix can also exert the characteristics of zirconium infrared emissivity and toughening. Therefore, the energy-saving kiln mouth castable provided by the present invention can synergistically achieve low thermal conductivity and high infrared emissivity, greatly reducing the energy consumption of the kiln mouth area of the cement kiln.
[0027] 4. The energy-saving lightweight cement kiln castable prepared by the present invention has been tested: the apparent porosity is 30-40%; the bulk density is 2.2-2.6 g / cm 3 ; The room temperature flexural strength at 110℃×24h is 4-9 MPa; The room temperature flexural strength at 1600℃×3h is 30-45MPa; The thermal conductivity at 1200℃ is 0.8-1.4 W / (m·K), and the average emissivity in the 0.76~2.5μm band at room temperature is 60-78%. The process of the present invention is simple, and the prepared infrared radiation castable for cement kiln mouth has the characteristics of high strength, good toughness, low thermal conductivity, high thermal reflectivity, and excellent thermal shock stability. It greatly improves the service life of kiln mouth refractory materials while reducing heat loss, and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1The average room temperature emissivity in the 0.76-2.5 μm band of the energy-saving lightweight cement kiln mouth castable prepared in Example 2 of the present invention and other refractory materials prepared by the same process. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0030] To avoid repetition, the materials involved in this specific implementation are first described uniformly as follows and will not be described in detail in the examples.
[0031] An energy-saving lightweight cement kiln mouth castable comprises the following components in parts by mass: 60-70 parts of lightweight lanthanum aluminate-mullite aggregate, 5-10 parts of silicon carbide fine powder, 8-12 parts of alumina fine powder, 4-8 parts of plate-shaped corundum fine powder, 1-3 parts of α-Al2O3 micropowder, 1-6 parts of lanthanum zirconate fine powder, 4-6 parts of calcium aluminate cement, 0.1-0.2 parts of water reducer and 5-6 parts of water.
[0032] Furthermore, the particle gradation of the lightweight lanthanum aluminate-mullite aggregate is: the particle size of 3-5 mm accounts for 40-50wt% of the lightweight lanthanum aluminate-mullite aggregate, the particle size of 1-3 mm accounts for 25-40wt% of the lightweight lanthanum aluminate-mullite aggregate, and the particle size of 0.1-1 mm accounts for 10-25wt% of the lightweight lanthanum aluminate-mullite aggregate; the porosity of the lightweight lanthanum aluminate-mullite aggregate is ≥50%, the average pore size is 2-20 μm, and the lanthanum aluminate content is ≥50wt%.
[0033] Furthermore, the particle size of the silicon carbide fine powder is ≤0.088 mm, and the SiC content of the silicon carbide fine powder is ≥90 wt%.
[0034] Furthermore, the particle size of the alumina fine powder is ≤0.088 mm, and the Al2O3 content in the alumina fine powder is ≥60 wt%.
[0035] Furthermore, the particle size of the plate-like corundum fine powder is ≤0.088 mm, and the Al2O3 content in the plate-like corundum fine powder is ≥99wt%.
[0036] Furthermore, the particle size of the α-Al2O3 micropowder is ≤2μm, and the Al2O3 content in the α-Al2O3 micropowder is ≥98wt%.
[0037] Furthermore, the particle size of the lanthanum zirconate fine powder is ≤ 88 μm, and the La2Zr2O7 content in the lanthanum zirconate fine powder is ≥ 99 wt%.
[0038] Furthermore, the Al2O3 content in the calcium aluminate cement is ≥71wt%.
[0039] Furthermore, the water reducing agent is one of sodium tripolyphosphate, sodium hexametaphosphate, FS10 or FS20.
[0040] A method for preparing an energy-saving lightweight cement kiln mouth castable comprises the following steps: Step 1, 4 to 12 parts of mullite fine powder, 1 to 3 parts of mullite micropowder, 2 to 6 parts of lanthanum aluminate fine powder, and 4 to 12 parts of dextrin are mixed, and ball-milled for 4 to 8 hours to obtain ball-milled powder; 6 to 10 parts of water are added to the ball-milled powder, granulated to obtain prefabricated spherical aggregates of different particle sizes, and dried at 110° C. for 24 to 36 hours; and the dried spherical aggregates are calcined under certain conditions, sieved, and lightweight lanthanum aluminate-mullite aggregates are obtained.
[0041] Step 2: first use 60-70 parts of lightweight lanthanum aluminate-mullite aggregate, 5-10 parts of silicon carbide fine powder, 8-12 parts of alumina fine powder, 4-8 parts of plate-shaped corundum fine powder, 1-3 parts of α-Al2O3 fine powder, 1-6 parts of lanthanum zirconate fine powder, and 4-6 parts of calcium aluminate cement as raw materials, add 0.1-0.2 parts of water reducer to the raw materials, mix well, then add 5-6 parts of water to the raw materials, stir well, shape, cure for 2-3 days, demold, and bake to obtain energy-saving lightweight cement kiln mouth castable.
[0042] Furthermore, in the step 1, the Al2O3 content in the mullite fine powder is ≤70wt%; the Al2O3 content in the mullite micropowder is ≤70wt%.
[0043] Furthermore, in step 1, the particle size of the prefabricated spherical aggregate is 5-3 mm, 3-1 mm and 1-0 mm.
[0044] Furthermore, in step 1, the calcination temperature is 1200-1400° C., and the calcination time is 3-8 hours.
[0045] Example 1.
[0046] An energy-saving lightweight cement kiln mouth castable and preparation method thereof: The preparation method of lightweight lanthanum aluminate-mullite aggregate is as follows: 4 parts of mullite fine powder, 1 part of mullite micropowder, 3 parts of lanthanum aluminate fine powder and 4 parts of dextrin are mixed, and ball-milled for 4 hours to obtain ball-milled powder; 6 parts of water are added to the ball-milled powder, granulated, and prefabricated spheres with particle sizes of 5-3 mm, 3-1 mm and 1-0 mm are respectively obtained, and dried at 110° C. for 24 hours; and the dried prefabricated spheres are calcined at 1400° C. for 5 hours, crushed, ball-milled and sieved to obtain lightweight lanthanum aluminate-mullite aggregate.
[0047] The preparation method of energy-saving lightweight cement kiln castable is as follows: first, 60 parts of lightweight lanthanum aluminate-mullite aggregate, 5 parts of silicon carbide fine powder, 10 parts of alumina fine powder, 6 parts of plate-shaped corundum fine powder, 1 part of α-Al2O3 fine powder, 6 parts of lanthanum zirconate fine powder, and 6 parts of calcium aluminate cement are used as raw materials, 0.2 parts of FS10 of the raw materials are added, and then 6 parts of water of the raw materials are added after mixing evenly, stirring evenly, molding, curing for 2 days, demolding, and baking to obtain energy-saving lightweight cement kiln castable.
[0048] The energy-saving lightweight cement kiln castable prepared in this embodiment is tested: the apparent porosity is 30%; the bulk density is 2.6 g / cm 3 ; The room temperature flexural strength at 110℃×24h is 9 MPa; the room temperature flexural strength at 1600℃×3h is 45MPa; the thermal conductivity at 1200℃ is 1.4 W / (m·K), and the average emissivity in the 0.76~2.5μm band at room temperature is 60%.
[0049] Example 2.
[0050] An energy-saving lightweight cement kiln mouth castable and preparation method thereof: The preparation method of lightweight lanthanum aluminate-mullite aggregate is as follows: firstly, 10 parts of mullite fine powder, 3 parts of mullite micro powder, 6 parts of lanthanum aluminate fine powder and 12 parts of dextrin are mixed, and ball-milled for 8 hours to obtain ball-milled powder; then, 10 parts of water are added to the ball-milled powder, granulated to obtain prefabricated spheres with particle sizes of 5-3 mm, 3-1 mm and 1-0 mm, and dried at 110° C. for 36 hours; then, the dried prefabricated spheres are calcined at 1200° C. for 5 hours, crushed and ball-milled to obtain lightweight lanthanum aluminate-mullite aggregate.
[0051] The preparation method of energy-saving lightweight cement kiln castable is as follows: first, 70 parts of lightweight lanthanum aluminate-mullite aggregate, 5 parts of silicon carbide fine powder, 11 parts of alumina fine powder, 8 parts of plate-shaped corundum fine powder, 3 parts of α-Al2O3 micropowder, 4 parts of lanthanum zirconate fine powder, and 5 parts of calcium aluminate cement are used as raw materials, and 0.2 parts of sodium tripolyphosphate are added to the raw materials, and then 5 parts of water are added to the raw materials after mixing evenly, stirring evenly, molding, curing for 3 days, demolding, and baking to obtain energy-saving lightweight cement kiln castable.
[0052] The energy-saving lightweight cement kiln castable prepared in this embodiment is tested: the apparent porosity is 40%; the bulk density is 2.2 g / cm 3 ; The room temperature flexural strength at 110℃×24h is 4 MPa; the room temperature flexural strength at 1600℃×3h is 30MPa; the thermal conductivity at 1200℃ is 0.8 W / (m·K), and the average emissivity in the 0.76~2.5μm band at room temperature is 78%.
[0053] Example 3.
[0054] Energy-saving lightweight cement kiln mouth castable and preparation method thereof: The preparation method of lightweight lanthanum aluminate-mullite aggregate is as follows: first, 8 parts of mullite fine powder, 2 parts of mullite micropowder, 4 parts of lanthanum aluminate fine powder and 8 parts of dextrin are mixed, and ball-milled for 8 hours to obtain ball-milled powder; then, 7 parts of water are added to the ball-milled powder, granulated to obtain prefabricated spheres with particle sizes of 5-3 mm, 3-1 mm and 1-0 mm, and dried at 110° C. for 36 hours; then, the dried prefabricated spheres are calcined at 1300° C. for 5 hours, crushed and ball-milled to obtain lightweight lanthanum aluminate-mullite aggregate.
[0055] The preparation method of energy-saving lightweight cement kiln castable is as follows: first, 65 parts of lightweight lanthanum aluminate-mullite aggregate, 8 parts of silicon carbide fine powder, 9 parts of alumina fine powder, 6 parts of plate-shaped corundum fine powder, 2 parts of α-Al2O3 micropowder, 4 parts of lanthanum zirconate fine powder, and 4 parts of calcium aluminate cement are used as raw materials, and 0.2 parts of sodium tripolyphosphate are added to the raw materials, and then 5 parts of water are added to the raw materials after mixing evenly, stirring evenly, molding, curing for 3 days, demolding, and baking to obtain energy-saving lightweight cement kiln castable.
[0056] The energy-saving lightweight cement kiln castable prepared in this embodiment has an apparent porosity of 35% and a bulk density of 2.4 g / cm 3 ; The room temperature flexural strength at 110℃×24h is 6 MPa; the room temperature flexural strength at 1600℃×3h is 37 MPa; the thermal conductivity at 1200℃ is 1.1 W / (m·K), and the average emissivity in the 0.76~2.5μm band at room temperature is 69%.
[0057] Example 4.
[0058] Energy-saving lightweight cement kiln mouth castable and preparation method thereof: The preparation method of alumina-lanthanum hexaaluminate composite fine powder is as follows: first, 6 parts of plate-like corundum fine powder, 2 parts of mullite micropowder, 3 parts of lanthanum aluminate fine powder and 9 parts of dextrin are mixed, and ball-milled for 7 hours to obtain ball-milled powder; then, 9 parts of water are added to the ball-milled powder, granulated to obtain prefabricated spheres with particle sizes of 5-3 mm, 3-1 mm and 1-0 mm, and dried at 110° C. for 36 hours; then, the dried prefabricated spheres are calcined at 1250° C. for 7 hours, crushed, and ball-milled to obtain lightweight lanthanum aluminate-mullite aggregate.
[0059] The preparation method of energy-saving lightweight cement kiln castable is as follows: first, 62 parts of lightweight lanthanum aluminate-mullite aggregate, 8 parts of silicon carbide fine powder, 11 parts of special-grade alumina fine powder, 5 parts of plate-shaped corundum fine powder, 1 part of α-Al2O3 micropowder, 3 parts of lanthanum zirconate fine powder, and 5 parts of calcium aluminate cement are used as raw materials, 0.2 parts of FS20 of the raw materials are added, and after mixing evenly, 6 parts of water of the raw materials are added, stirred evenly, formed, cured for 3 days, demolded, and baked to obtain energy-saving lightweight cement kiln castable.
[0060] The energy-saving lightweight cement kiln castable prepared in this embodiment has an apparent porosity of 33% and a bulk density of 2.5 g / cm 3 ; The room temperature flexural strength at 110℃×24h is 7 MPa; the room temperature flexural strength at 1600℃×3h is 40 MPa; the thermal conductivity at 1200℃ is 1.2 W / (m·K), and the average emissivity in the 0.76~2.5μm band at room temperature is 72%.
[0061] Comparative example 1.
[0062] A cement kiln mouth castable and a preparation method thereof: firstly, 60 parts of mullite lightweight aggregate, 5 parts of silicon carbide fine powder, 10 parts of alumina fine powder, 6 parts of plate-shaped corundum fine powder, 1 part of α-Al2O3 micropowder, 6 parts of lanthanum zirconate fine powder and 6 parts of calcium aluminate cement are used as raw materials, 0.2 parts of FS10 of the raw materials are added, and after mixing evenly, 6 parts of water of the raw materials are added, stirred evenly, formed, cured for 2 days, demoulded and baked to obtain an energy-saving lightweight cement kiln mouth castable.
[0063] The energy-saving lightweight cement kiln mouth castable prepared in this comparative example was tested: the apparent porosity was 18%; the volume density was 2.9 g / cm3; the room-temperature flexural strength at 110°C×24h was 10 MPa; the room-temperature flexural strength at 1600°C×3h was 50 MPa; the thermal conductivity at 1200°C was 2.3 W / (m·K), and the average emissivity in the 0.76~2.5μm band at room temperature was 25%.
[0064] Comparative example 2.
[0065] An energy-saving lightweight cement kiln mouth castable and preparation method thereof: The preparation method of lightweight lanthanum aluminate-mullite aggregate is as follows: 4 parts of mullite fine powder, 1 part of mullite micropowder, 3 parts of lanthanum aluminate fine powder and 4 parts of dextrin are mixed, and ball-milled for 4 hours to obtain ball-milled powder; 6 parts of water are added to the ball-milled powder, granulated, and prefabricated spheres with particle sizes of 5-3 mm, 3-1 mm and 1-0 mm are respectively obtained, and dried at 110° C. for 24 hours; and the dried prefabricated spheres are calcined at 1400° C. for 5 hours, crushed, ball-milled and sieved to obtain lightweight lanthanum aluminate-mullite aggregate.
[0066] The preparation method of energy-saving lightweight cement kiln castable is as follows: first, 60 parts of lightweight lanthanum aluminate-mullite aggregate, 5 parts of silicon carbide fine powder, 10 parts of alumina fine powder, 12 parts of plate-shaped corundum fine powder, 1 part of α-Al2O3 micropowder, and 6 parts of calcium aluminate cement are used as raw materials, and 0.2 parts of FS10 of the raw materials are added, and then 6 parts of water of the raw materials are added after mixing evenly, stirring evenly, molding, curing for 2 days, demolding, and baking to obtain energy-saving lightweight cement kiln castable.
[0067] The energy-saving lightweight cement kiln castable prepared in this comparative example was tested: the apparent porosity was 28%; the bulk density was 2.7 g / cm 3 ; The room temperature flexural strength at 110℃×24h is 8 MPa; the room temperature flexural strength at 1600℃×3h is 42 MPa; the thermal conductivity at 1200℃ is 1.7 W / (m·K), and the average emissivity in the 0.76~2.5μm band at room temperature is 50%.
Claims
1. An energy-saving lightweight cement kiln mouth castable, characterized in that: The invention comprises the following components in parts by weight: 60-70 parts of lightweight lanthanum aluminate-mullite aggregate, 5-10 parts of silicon carbide fine powder, 8-12 parts of alumina fine powder, 4-8 parts of plate-like corundum fine powder, 1-3 parts of α-Al2O3 fine powder, 1-6 parts of lanthanum zirconate fine powder, 4-6 parts of calcium aluminate cement, 0.1-0.2 parts of water reducer and 5-6 parts of water.
2. An energy-saving lightweight cement kiln castable according to claim 1, characterized in that: The particle gradation of the lightweight lanthanum aluminate-mullite aggregate is as follows: particles with a particle size of 3-5 mm account for 40-50 wt% of the lightweight lanthanum aluminate-mullite aggregate, particles with a particle size of 1-3 mm account for 25-40 wt% of the lightweight lanthanum aluminate-mullite aggregate, and particles with a particle size of 0.1-1 mm account for 10-25 wt% of the lightweight lanthanum aluminate-mullite aggregate; the porosity of the lightweight lanthanum aluminate-mullite aggregate is ≥50%, the average pore size is 2-20 μm, and the lanthanum aluminate content is ≥50 wt%.
3. According to the energy-saving lightweight cement kiln castable according to claim 1, it is characterized in that: The particle size of the silicon carbide fine powder is ≤0.088 mm, and the SiC content of the silicon carbide fine powder is ≥90 wt %; the particle size of the alumina fine powder is ≤0.088 mm, and the Al2O3 content of the alumina fine powder is ≥60 wt %.
4. According to the energy-saving lightweight cement kiln castable according to claim 1, it is characterized in that: The particle size of the plate-like corundum fine powder is ≤0.088 mm, and the Al2O3 content in the plate-like corundum fine powder is ≥99wt%; the particle size of the α-Al2O3 micropowder is ≤2μm, and the Al2O3 content in the α-Al2O3 micropowder is ≥98wt%.
5. According to the energy-saving lightweight cement kiln castable according to claim 1, it is characterized in that: The particle size of the lanthanum zirconate fine powder is ≤ 88 μm, and the La2Zr2O7 content in the lanthanum zirconate fine powder is ≥ 99 wt%.
6. The energy-saving lightweight cement kiln castable according to claim 1, characterized in that: The Al2O3 content in the calcium aluminate cement is ≥71wt%.
7. An energy-saving lightweight cement kiln castable according to claim 1, characterized in that: The water reducing agent is one of sodium tripolyphosphate, sodium hexametaphosphate, FS10 or FS20.
8. A method for preparing an energy-saving lightweight cement kiln castable, characterized in that: The steps include: Step 1, firstly mix 4-12 parts of mullite fine powder, 1-3 parts of mullite micropowder, 2-6 parts of lanthanum aluminate fine powder, and 4-12 parts of dextrin, and ball-mill for 4-8 hours to obtain ball-milled powder; then add 6-10 parts of water to the ball-milled powder, granulate, obtain prefabricated spherical aggregate, and dry at 110° C. for 24-36 hours; then calcine the dried spherical aggregate under certain conditions, sieve, and obtain lightweight lanthanum aluminate-mullite aggregate; Step 2: first use 60-70 parts of lightweight lanthanum aluminate-mullite aggregate, 5-10 parts of silicon carbide fine powder, 8-12 parts of alumina fine powder, 4-8 parts of plate-shaped corundum fine powder, 1-3 parts of α-Al2O3 micropowder, 1-6 parts of lanthanum zirconate fine powder, and 4-6 parts of calcium aluminate cement as raw materials, add 0.1-0.2 parts of water reducer to the raw materials, mix well, then add 5-6 parts of water to the raw materials, stir well, shape, cure for 2-3 days, demold, and bake to obtain energy-saving lightweight cement kiln mouth castable.
9. The method for preparing an energy-saving lightweight cement kiln castable according to claim 8, characterized in that: In the step 1, the Al2O3 content in the mullite fine powder is ≤70wt%; the Al2O3 content in the mullite micropowder is ≤70wt%.
10. The method for preparing an energy-saving lightweight cement kiln castable according to claim 8, characterized in that: In the step 1, the particle sizes of the prefabricated spherical aggregate are 5-3 mm, 3-1 mm and 1-0 mm; the calcination temperature is 1200-1400° C., and the calcination time is 3-8 hours.
Citation Information
Patent Citations
Medium-density brick used for rotary kiln and preparation method thereof
CN103058682A
Heat barrier and heat radiation complex function based aluminum oxide pouring material for saving energy in high-temperature environment
CN104446524A
Infrared radiation castable for kilneye of cement kiln and preparation method of infrared radiation castable
CN114133254A
Vacuum and heat radiation prevention synergistic heat preservation metallurgical ladle
CN114749645A
Lightweight thermal insulation castable for cement kiln head cover
CN114890801A