Disulfide compound, preparation method and application thereof, and method for recovering precious metal through solvent extraction

By designing a structurally optimized disulfide compound, the efficiency and acid resistance of existing sulfide extractants in gold and palladium recovery are solved, and the recovery of precious metal ions is achieved efficient and selective, and the recovery of its in-depth analysis is carried out. Potential and reuse capabilities in industrial applications.

CN118908867APending Publication Date: 2024-11-08HUNAN INSTITUTE OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410968643.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing sulfide extractors have problems such as slow extraction kinetics, low extraction amount, poor acid resistance and poor taste in recovering gold and palladium, which limits their industrial application potential.

Method used

A disulfide compound was designed, and its structure was controlled by introducing two sulfur atoms and connecting them through ethyl groups to improve the complexing capacity with noble metal ions, and was recovered by solvent extraction. This compound is prepared by reaction with 1,2-bis(carboxymethylthio)-ethane and alkyl alcohol, and is characterized by high efficiency, good selectivity and reusability.

Benefits of technology

It realizes the recycling of high-efficiency and selectivity of precious metal ions (Au(III) and Pd(II)), high extraction saturation capacity, and high selectivity and high performance for Au(III) and Pd(II) at low acidity. The extraction rate proves its suitable performance for industrial application and reuse.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908867A_ABST
    Figure CN118908867A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of recovery of precious metals through a solvent extraction method, and particularly relates to a disulfide compound, a preparation method and application thereof, and a method for recovering precious metals through solvent extraction. The disulfide compound provided by the invention has a structure as shown in a formula 1. According to the disulfide compound provided by the invention, two sulfur atoms are introduced into the structure of the compound, the two sulfur atoms are connected through an ethyl group, an R group is used as an ester alkyl substituent group to be connected with two sulfur groups, and meanwhile, the ester alkyl chain length of the compound is controlled; the complexing ability of the chemical with the structure as shown in the formula 1 serving as an extracting agent and precious metal ions can be remarkably improved, so that the precious metal ions (Au (III) and Pd (II)) can be efficiently and selectively recycled from an aqueous solution. According to the technical scheme, the preparation method of the disulfide compound is simple in synthesis, high in yield and suitable for industrial application. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of recovering precious metals by solvent extraction, and specifically relates to a disulfide compound and a preparation method and application thereof, and a method for recovering precious metals by solvent extraction. Background Art

[0002] Precious metals such as gold and palladium are widely used in jewelry, corrosion-resistant materials, electronic technology, and chemical catalysts due to their luster, ductility, non-corrosiveness, and high stability. However, as a non-renewable resource, precious metals such as gold and palladium are rarely distributed worldwide, so secondary recycling is particularly important. Therefore, the selective recovery of gold and palladium ions from industrial wastewater has attracted the attention of many scientific researchers.

[0003] Solvent extraction has become an important means of recovering precious metals from wastewater due to its advantages of simple operation, low energy consumption, easy industrialization, and the ability to selectively separate target metals. At present, the commonly used extractants for recovering precious metals by solvent extraction include thioether extractants.

[0004] In general, alkyl sulfides have the characteristics of small molecular weight and simple preparation process, such as di-n-hexyl sulfide (DHS) and di-n-octyl sulfide (DOS), which have commercial application potential and can well separate Pd(II) from mixed media. However, there are disadvantages such as slow extraction kinetics, low extraction volume and poor acid resistance. In order to overcome these problems, branched and electron-withdrawing groups are introduced into the linear chain of sulfide extractants to improve stability. Oxygen-containing functional groups have better affinity for Au(III) and theoretically make it easier to coordinate with Au(III) during the extraction process. In addition, the taste of traditional sulfide extractants is poor, which limits their potential for industrial application. Summary of the invention

[0005] The purpose of the present invention is to provide a disulfide compound and a preparation method and application thereof, and a method for recovering precious metals by solvent extraction. When the disulfide compound provided by the present invention is used as an extractant for recovering precious metals in an aqueous solution by solvent extraction, it has the advantages of high extraction efficiency, good selectivity, extraction rate and large saturation capacity, and can be reused, and is suitable for industrial promotion and application.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] The present invention provides a disulfide compound having a structure shown in Formula 1:

[0008]

[0009] In formula 1: R is a C1-10 alkyl group.

[0010] Preferably, R is ethyl or n-pentyl.

[0011] The present invention provides a method for preparing the disulfide compound described in the above technical solution, comprising the following steps:

[0012] 1,2-bis(carboxymethylthio)-ethane, thionyl chloride and an organic solvent are mixed to carry out an acyl chloride reaction to obtain an acyl chloride product; the acyl chloride product has a structure shown in Formula 2:

[0013]

[0014] The acyl chloride product, organic base and alkyl alcohol are mixed for substitution reaction to obtain a disulfide compound with a structure shown in Formula 1; the alkyl alcohol has a structure shown in Formula 3: R-OH Formula 3.

[0015] The present invention provides the use of the disulfide compound described in the above technical solution or the disulfide compound prepared by the preparation method described in the above technical solution in recovering precious metals by a solvent extraction method.

[0016] Preferably, the noble metal includes gold and / or palladium.

[0017] The present invention provides a method for recovering precious metals by solvent extraction, comprising the following steps:

[0018] The extractant organic phase solution and the aqueous phase solution containing precious metals are mixed for extraction to obtain an extracted organic phase enriched with precious metals and a raffinate aqueous phase; the extractant organic phase solution comprises an extractant and an organic diluent, and the extractant is the disulfide compound described in the above technical solution or the disulfide compound prepared by the preparation method described in the above technical solution; the aqueous phase solution containing precious metals is an acidic solution.

[0019] Preferably, the organic diluent includes one or more of kerosene, n-hexane, toluene, xylene, chloroalkane and butyl acetate;

[0020] The molar concentration of the extractant in the extractant organic phase solution is 2 mmol / L.

[0021] Preferably, the aqueous solution containing precious metals comprises precious metals, water and inorganic strong acid; in the aqueous solution containing precious metals: the molar concentration of the precious metals is 0.25 to 7 mmol / L, and the molar concentration of the inorganic strong acid is 0.1 to 4 mol / L.

[0022] Preferably, the volume ratio of the organic phase solution of the extractant to the aqueous phase solution containing the precious metals is 1:9 to 9:1; the extraction temperature is room temperature, and the extraction time is ≥15 min.

[0023] Preferably, after obtaining the extracted organic phase enriched in precious metals, the method further comprises: mixing the extracted organic phase enriched in precious metals and a stripping agent aqueous phase solution for stripping to obtain an extracted aqueous phase enriched in precious metals and a residual organic phase; the stripping agent aqueous phase solution comprises a stripping agent and water, the stripping agent comprises oxalic acid, NH3 or thiourea, or the stripping agent is a mixture of thiourea and HCl.

[0024] The present invention provides a disulfide compound having a structure shown in Formula 1. The disulfide compound provided by the present invention can significantly improve the complexing ability of the chemical with the structure shown in Formula 1 as an extractant with precious metal ions by introducing two sulfur atoms into the structure of the compound, connecting the two sulfur atoms through an ethyl group, and connecting the two sulfurs through an R group as an ester alkyl substituent, while controlling the ester alkyl chain length of the compound, so as to efficiently and selectively recover precious metal ions (Au (III) and Pd (II)) from an aqueous solution. It can be seen from the results of the embodiment that the disulfide compound with the structure shown in Formula 1 provided by the present invention is used as an extractant: 1,2-dichloroethane is used as a diluent, and 2mmol / L of the extractant extracts 1mmol / L of metal ions under 0.1mol / LHCl, and the equilibrium time required for extracting gold is 2h, and the equilibrium time required for extracting palladium is 30min, indicating that the extraction efficiency is high. The saturated capacities of SS-C2 and SS-C5 for extracting Au(III) are 750.60 mg / g and 557.98 mg / g, respectively, and the saturated capacities for extracting Pd(II) are 500.17 mg / g and 484.87 mg / g, respectively. At the same time, through the study of selectivity experiments, it was found that the chemical with the structure shown in Formula 1 under low acidity has high selectivity and high extraction rate for Au(III) and Pd(II) as an extractant. Increasing the concentration of the extractant will increase the extraction rate for Au(III) and Pd(II) without extracting metal impurities, indicating that the extractant has excellent selectivity. The present invention proves that the extractant has the property of being reusable by stripping with an acidic thiourea solution.

[0025] The present invention provides a method for preparing the disulfide compound described in the above technical solution. The present invention selects 1,2-bis(carboxymethylthio)-ethane as a raw material, reacts with an alkyl alcohol, and synthesizes a novel disulfide extractant with different ester alkyl chain lengths (including 1,2-(carboxyethylmethylthio)-ethane (denoted as SS-C2) and 1,2-bis(carboxypentylmethylthio)-ethane (denoted as SS-C5)). The preparation method provided by the present invention has simple synthesis, high yield, and is suitable for industrial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The synthetic route of the extractant in the embodiment of the present invention;

[0027] Figure 2is the effect of diluent on the extraction rate of Au(III) and Pd(II);

[0028] Figure 3 is the effect of HCl concentration on the extraction of Au(III) and Pd(II);

[0029] Figure 4 is the extraction kinetics of Au(III) and Pd(II);

[0030] Figure 5 is the extraction capacity of the extractant for Au(III) and Pd(II);

[0031] Figure 6 Job's diagram of extractant-Au(III) and extractant-Pd(II) complexes;

[0032] Figure 7 H + and Cl- concentration on the extraction of Au(III) and Pd(II);

[0033] Figure 8 It is the ultraviolet absorption peak of SS-C2 and SS-C5 complexes with gold and palladium;

[0034] Fig. 9 Extraction efficiency of SS-C2 and SS-C5 for simulated mixed metal ion solution. DETAILED DESCRIPTION

[0035] The present invention provides a disulfide compound having a structure shown in Formula 1:

[0036]

[0037] In formula 1: R is a C1-10 alkyl group.

[0038] In the present invention, R is preferably a C2-8 alkyl group, more preferably a C2-6 alkyl group, further preferably an ethyl group, a propyl group, a butyl group, a pentyl group or a hexyl group, and specifically preferably an ethyl group or an n-pentyl group.

[0039] The present invention provides a method for preparing the disulfide compound described in the above technical solution, comprising the following steps:

[0040] 1,2-bis(carboxymethylthio)-ethane, thionyl chloride and an organic solvent are mixed to carry out an acyl chloride reaction to obtain an acyl chloride product; the acyl chloride product has a structure shown in Formula 2:

[0041]

[0042] The acyl chloride product, organic base and alkyl alcohol are mixed for substitution reaction to obtain a disulfide compound with a structure shown in Formula 1; the alkyl alcohol has a structure shown in Formula 3: R-OH Formula 3.

[0043] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.

[0044] The present invention mixes 1,2-bis(carboxymethylthio)-ethane, thionyl chloride and an organic solvent (hereinafter referred to as the first organic solvent) to carry out an acyl chloride reaction to obtain an acyl chloride product; the acyl chloride product has a structure shown in Formula 2. In the present invention, the mass ratio of the 1,2-bis(carboxymethylthio)-ethane to the volume of the thionyl chloride is preferably 6.3g:8mL. The first organic solvent is preferably N,N-dimethylformamide (DMF). The present invention has no special requirements for the amount of the first organic solvent, as long as the acyl chloride reaction is carried out smoothly. The temperature of the acyl chloride reaction is preferably 50 to 60°C, and the time is preferably 1 to 3h. After the acyl chloride reaction is completed, the present invention preferably evaporates the obtained acyl chloride reaction liquid to obtain the acyl chloride product. The evaporation is preferably rotary evaporation. The present invention preferably removes unreacted thionyl chloride and organic solvent by evaporation. The evaporated product is preferably cooled in an ice bath.

[0045] After obtaining the acyl chloride product, the present invention mixes the acyl chloride product, an organic base and an alkyl alcohol for a substitution reaction to obtain a disulfide compound with a structure shown in Formula 1; the alkyl alcohol has a structure shown in Formula 3: R-OH Formula 3. In the present invention, the organic base is preferably triethylamine. The alkyl alcohol is preferably ethanol or n-pentanol. When the alkyl alcohol is preferably n-pentanol, the mixed raw material also includes a second organic solvent, and the second organic solvent is preferably 1,4-dioxane. The molar ratio of the mass of the 1,2-bis(carboxymethylthio)-ethane to the alkyl alcohol is preferably 1:2. The present invention has no special requirements for the amount of the triethylamine and the organic solvent, as long as the substitution reaction is smoothly carried out. The temperature of the substitution reaction is preferably 60°C, and the time is preferably 12h. After the substitution reaction is completed, the present invention preferably evaporates the obtained substitution reaction liquid, obtains the evaporated product, and dissolves it in ethyl acetate for solid-liquid separation, and the obtained liquid phase solution is washed and dried in sequence to obtain an ethyl acetate solution after impurities are removed; the ethyl acetate solution after impurities is desolventized to obtain a disulfide compound with a structure shown in Formula 1. The solvent used for the washing is preferably NaHCO3 solution and water, the washing is preferably carried out in sequence with NaHCO3 solution and water, the number of washings with NaHCO3 solution is preferably 3 times, the number of washings with water is preferably 3 times, and the reagent used for the drying is preferably anhydrous sodium sulfate. The disulfide compound of the structure shown in Formula 1 is a brown liquid.

[0046] The present invention provides the use of the disulfide compound described in the above technical solution or the disulfide compound prepared by the preparation method described in the above technical solution in recovering precious metals by a solvent extraction method.

[0047] In the present invention, the noble metal includes gold and / or palladium. The noble metal is preferably a noble metal ion. The noble metal ion is preferably Au(III) and / or Pd(II).

[0048] The present invention provides a method for recovering precious metals by solvent extraction, comprising the following steps:

[0049] The extractant organic phase solution and the aqueous phase solution containing precious metals are mixed for extraction to obtain an extracted organic phase enriched with precious metals and a raffinate aqueous phase; the extractant organic phase solution comprises an extractant and an organic diluent, and the extractant is the disulfide compound described in the above technical solution or the disulfide compound prepared by the preparation method described in the above technical solution; the aqueous phase solution containing precious metals is an acidic solution.

[0050] In the present invention, the organic diluent includes one or more of kerosene, n-hexane, toluene, xylene, chloroalkanes and butyl acetate, more preferably chloroalkanes or butyl acetate. The chloroalkanes preferably include one or more of dichloromethane, chloroform and 1,2-dichloroethane. The butyl acetate is specifically preferably n-butyl acetate. The organic diluent is most preferably 1,2-dichloroethane. The molar concentration of the extractant in the extractant organic phase solution is preferably 2mmol / L.

[0051] In the present invention, the aqueous solution containing precious metals comprises precious metals, water and inorganic strong acid. The inorganic strong acid is preferably HCl. In the aqueous solution containing precious metals: the molar concentration of the precious metal is preferably 0.25-7 mmol / L, more preferably 0.5-4.7 mmol / L, and most preferably 1-2 mmol / L. In a specific embodiment of the present invention, when the precious metal in the aqueous solution containing precious metals is Au(III), the molar concentration of Au(III) is preferably 0.25-7 mmol / L, and most preferably 1-2 mmol / L. When the precious metal in the aqueous solution containing precious metals is Pd(II), the molar concentration of Pd(II) is preferably 0.5-6 mmol / L, and most preferably 1-2 mmol / L. The molar concentration of the inorganic strong acid is preferably 0.1-4 mol / L, and more preferably 0.1 mol / L.

[0052] In the present invention, the volume ratio of the organic phase solution of the extractant to the aqueous phase solution containing the precious metal is preferably 1:9 to 9:1, more preferably 1:5 to 5:1, and most preferably 1:1.

[0053] In the present invention, the extraction temperature is room temperature, specifically preferably 25°C, and the time is preferably ≥15min. In a specific embodiment of the present invention, when the precious metal in the aqueous solution containing precious metals is Au(III), the extractant in the extractant organic solution is SS-C2, and the extraction time is preferably 30min. When the precious metal in the aqueous solution containing precious metals is Au(III), the extractant in the extractant organic solution is SS-C5, and the extraction time is preferably 2h. When the precious metal in the aqueous solution containing precious metals is Pd(II), the extractant in the extractant organic solution is SS-C2, and the extraction time is preferably 15min. When the precious metal in the aqueous solution containing precious metals is Pd(II), the extractant in the extractant organic solution is SS-C5, and the extraction time is preferably 30min.

[0054] In the present invention, after obtaining the extracted organic phase enriched in precious metals, the present invention preferably further comprises: mixing the extracted organic phase enriched in precious metals and a stripping agent aqueous phase solution for stripping to obtain an extracted aqueous phase enriched in precious metals and a residual organic phase; the stripping agent aqueous phase solution comprises a stripping agent and water, the stripping agent comprises oxalic acid, NH3 or thiourea, or the stripping agent is a mixture of thiourea and HCl.

[0055] In the present invention, the molar concentration of the stripping agent in the stripping agent aqueous solution is preferably 1 to 1.5 mol / L. In a specific embodiment of the present invention, when the stripping agent is preferably oxalic acid, the molar concentration of oxalic acid is preferably 1 mol / L. When the stripping agent is preferably NH3, the molar concentration of NH3 is preferably 1 mol / L. When the stripping agent is preferably thiourea, the molar concentration of thiourea is preferably 1 mol / L. When the stripping agent is preferably a mixture of thiourea and HCl, the molar concentration of thiourea is preferably 0.5 mol / L, and the molar concentration of HCl is preferably 1 mol / L.

[0056] In the present invention, the volume ratio of the precious metal-enriched extraction organic phase to the stripping agent aqueous phase solution is preferably 1:1.

[0057] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0058] The main reagents used in the following examples are shown in Table 1.

[0059] Table 1 Main reagents

[0060]

[0061]

[0062] Example 1

[0063] Reference Figure 1 The extractant is prepared by the synthetic route of the extractant shown:

[0064] The synthesis steps of 1,2-bis(carboxyethylmethylthio)-ethane (SS-C2) are as follows: 6.3g (30mmol, 1eq) of 1,2-bis(carboxymethylthio)-ethane, 8mL of dichlorothionyl and several drops of DMF are added to an eggplant-shaped bottle at room temperature, and the dichlorothionyl is removed after reacting at 60°C for 3h. The system is cooled in an ice bath, and then 8.3mL (60mmol, 2eq) of triethylamine and 8mL of anhydrous ethanol are slowly added to the cooled crude acyl chloride product while stirring, and then the temperature is raised to 90°C for reaction for 12h. After the reaction is completed, the excess anhydrous ethanol is removed by rotary evaporation, and then ethyl acetate is used as a solvent. After filtering, it is washed 3 times with a certain concentration of NaHCO3 solution, and then washed 3 times with water, and dried with anhydrous sodium sulfate. The product is obtained by rotary drying of ethyl acetate as a brown liquid. The yield is 6.01g, and the yield is 71%. 1 HNMR(400MHz,Chloroform-d)δ4.19(q,J=7.1Hz,4H),3.25(s,4H),2.89(s,4H),1.29(t,J=7.2Hz,6H).

[0065] The synthesis steps of 1,2-bis(carboxypentylmethylthio)-ethane (SS-C5) are the same as above, wherein the amount of n-pentanol used is 7.1 mL (60 mmol, 2 eq), and the reaction solvent is 1,4-dioxane. The product is a brown liquid. The yield is 5.79 g, and the yield is 55.14%. 1 HNMR(400MHz,Chloroform-d)δ4.12(t,J=6.8Hz,4H),3.25(s,4H),2.89(s,4H ),1.74-1.58(m,4H),1.34(dq,J=10.5,3.5Hz,8H),0.91(q,J=6.8,4.7Hz,6H).

[0066] The synthesis steps of diethyl 3,3'-dithiodipropionate (SS) are the same as above, wherein the amount of 3,3'-dithiodipropionic acid used is 2g (9.52mmol, 1eq), and the reaction solvent is anhydrous ethanol. The product is a light brown liquid. The yield is 1.72g, and the yield is 80%. 1 HNMR(400MHz,Chloroform-d)δ4.16(q,J=7.1Hz,4H),2.92(t,J=7.2Hz,4H),2.72(t,J=7.2Hz,4H),1.26(t,J=7.1Hz,6H).

[0067] Extraction experiment

[0068] Through liquid-liquid extraction experiments, the extraction performance of the synthetic extractant of Example 1 on Au (III) and Pd (II) was explored. Gold and palladium chlorides were dissolved in hydrochloric acid aqueous solution to prepare initial solutions with concentrations of 5mmol / L and 10mmol / L respectively, and the initial solutions were diluted to 1mmol / L for standby use. A certain amount of extractant was dissolved in a diluent to prepare an organic phase, and a single metal ion solution containing 1mmol / LAu (III) and 1mmol / LPd (II) was used as the aqueous phase for solvent extraction. Equal volumes (5mL each) of aqueous phase and organic phase were placed in a 50mL centrifuge tube, placed in a constant temperature oscillator and shaken at a speed of 230rmp for 12h. All extraction experiments were carried out at room temperature (25°C). After the extraction was completed, the two phases were separated and the metal ion concentration in the aqueous phase was determined by atomic absorption flame spectrometry (AAS). According to the mass conservation theory, the concentration of metal ions in the organic phase was determined by the difference in metal ion concentration in the aqueous phase before and after extraction. The present invention systematically studies the effects of factors such as diluent, extraction time, hydrochloric acid concentration, and extractant concentration on the extraction process, and further explores the ion selectivity of the extractant and the extraction mechanism.

[0069] The calculation equation for the extraction rate (E%) of metal ions is shown in Formula 1, and the calculation equation for the distribution ratio (D) is shown in Formula 2:

[0070]

[0071] In formula 1 and formula 2, C in and C eq are defined as the initial concentration and equilibrium concentration of metal ions in the aqueous phase, respectively.

[0072] Stripping experiment

[0073] After the extraction, the aqueous phase and the organic phase were separated, and the loaded organic phase (5 mL) containing the metal complex was stripped with a 1 mol / L HCl+0.5 mol / L thiourea mixed solution (5 mL) at 25°C and 230 rpm. After the stripping, the concentration of metal ions in the aqueous phase was detected by atomic absorption spectroscopy (AAS), and the organic phase entered the next extraction-stripping cycle after washing. The stripping rate was calculated as shown in Formula 3.

[0074]

[0075] In formula 3, C in,org Defined as the equilibrium concentration of metal ions in the organic phase; C eq,aq Defined as the metal ion concentration in the aqueous phase after stripping.

[0076] Results and Discussion

[0077] (1) Effect of diluent

[0078] Extraction efficiency is a standard for measuring the extraction effect and is a key parameter of extraction performance. The viscosity, polarity, boiling point and volatility of the diluent will affect the extraction efficiency. Therefore, the present invention first investigates the effect of the diluent on the extraction performance. Non-polar solvents (kerosene, n-hexane), medium polar solvents (toluene, xylene) and polar solvents (dichloromethane, chloroform, 1,2-dichloromethane and butyl acetate) are selected as diluents.

[0079] Prepare Au(III) and Pd(II) aqueous solutions with a hydrochloric acid concentration of 0.1 mol / L and a metal ion concentration of 1000 ppm. Use a pipette to transfer 20 mL of 1000 ppm Au(III) aqueous solution and 10 mL of 1000 ppm Pd(II) aqueous solution into two 100 mL volumetric flasks, add 0.1 mol / L hydrochloric acid, dilute and fix the volume to obtain Au(III) and Pd(II) aqueous solutions with a metal ion concentration of 200 ppm and 100 ppm (aqueous phase).

[0080] Add different masses of extractants into a 25 mL volumetric flask: SS-C2 13.3 mg, SS-C5 17.5 mg, and dilute to volume with different diluents to obtain an extractant (organic phase) with a concentration of 2 mmol / L.

[0081] Prepare several centrifuge tubes, transfer equal volumes (5 mL each) of aqueous phase and organic phase into the centrifuge tubes, shake at 25°C and 230 rpm for 6 h, then take the aqueous phase, filter it through a filter head, and perform atomic absorption analysis.

[0082] The extraction experiment was carried out under the conditions of extractant concentration of 2mmol / L, 0.1mol / L HCl, extraction time t=6h, extraction temperature T=25℃, [Au(III)]=[Pd(II)]=1mmol / L. The results are shown in Figure 2 As shown, Figure 2 (a) is the effect of diluent on Au(III) extraction rate. Figure 2 (b) shows the effect of diluent on the extraction rate of Pd(II). Figure 2It can be seen that the extraction efficiency of the same extractant in different diluents varies greatly, indicating that the diluent has a significant effect on the extraction of Au(III) and Pd(II). Except for the low extraction rate in chloroform (86.6%), SS-C2 has a high extraction rate (more than 95%) for Au(III) in the selected diluents; however, the extraction of Pd(II) is affected by the diluent, with the extraction rate of Pd(II) reaching more than 92% in chloroalkane diluents and poor extraction effect in other diluents, less than 40%. SS-C5 shows different performance. SS-C5 has a low extraction rate for Au(III), and the extraction effect in dichloromethane, 1,2-dichloroethane and n-butyl acetate is more than 94%; surprisingly, SS-C5 shows excellent extraction ability in the extraction process of Pd(II), with an extraction rate of up to 99% for Pd(II) in all the explored diluents. In general, SS-C2 and SS-C5 have good extraction effects on Au(III) and Pd(II), while SS shows poor extraction results. SS has a higher extraction rate for Au(III) in non-polar and weakly polar diluents. However, according to the phenomenon after extraction, when Au(III) was extracted with toluene, xylene, kerosene and n-hexane as diluents, the presence of elemental gold was found in the aqueous phase, indicating that a redox reaction occurred during the extraction process. This is because SS has a disulfide bond and weak antioxidant ability, which causes the gold ions in the aqueous phase to be reduced. The extraction rate of SS for Pd(II) is less than 50%, and the best effect is achieved in the diluent of chlorinated alkanes. This is the extraction effect of the extractant itself rather than the redox property of the extractant, because Pd(II) is not easily reduced.

[0083] In summary, the extractants (SS-C2 and SS-C5) provided by the present invention have the best extraction effect among the chlorinated alkane diluents. Since 1,2-dichloroethane has a higher boiling point, 1,2-dichloroethane is selected as the diluent of the system for subsequent experiments. Similarly, since SS will cause gold reduction during the extraction process and does not meet the selection criteria of the extractant, its subsequent extraction conditions are not investigated.

[0084] (2) Effect of hydrochloric acid concentration

[0085] Elucidating the effect of hydrochloric acid concentration on metal extraction is of great significance for industrial applications. To study the effect of hydrochloric acid concentration on extraction, the hydrochloric acid concentration was controlled in the range of 0.1 to 4 mol / L and extraction experiments were carried out. At the same time, in order to obtain obvious extraction rules, the initial concentration of palladium was increased to 2 mmol / L.

[0086] Prepare Au(III) and Pd(II) aqueous solutions with a hydrochloric acid concentration of 0.1 mol / L and a metal ion concentration of 1000 ppm. Use a pipette to transfer 20 mL of the 1000 ppm Au(III) aqueous solution into a 100 mL volumetric flask, add different volumes of concentrated hydrochloric acid, dilute and fix the volume to obtain Au(III) with a metal ion concentration of 200 ppm, and the hydrochloric acid concentrations are 0.1, 0.5, 1, 2, 3 and 4 mol / L, respectively; the preparation method of different hydrochloric acid concentrations of palladium is the same as above. Transfer 20 mL of the 1000 ppm Pd(II) aqueous solution and add different volumes of concentrated hydrochloric acid to adjust the hydrochloric acid concentration, dilute and fix the volume to obtain Pd(II) aqueous solutions with hydrochloric acid concentrations of 0.1, 0.5, 1, 2, 3 and 4 mol / L, respectively, and a metal ion concentration of 200 ppm.

[0087] Take 6 centrifuge tubes, add 5 mL of Au(III) aqueous solution with different hydrochloric acid concentrations to each centrifuge tube. Take another 6 centrifuge tubes, add 5 mL of Pd(II) aqueous solution with different acidity to each centrifuge tube.

[0088] Prepare the organic phase separately. Weigh 53.2 mg of extractant SS-C2 and dilute it to 100 mL with 1,2-dichloroethane to obtain an extractant with a concentration of 2 mmol / L. The preparation method of SS-C5 is the same as above, and the mass of the extractant is 70 mg.

[0089] 5 mL of the prepared extractant was transferred into each of the above centrifuge tubes, and the tubes were placed in a constant temperature water bath shaker at 25°C for 6 hours. After the extraction was completed, the upper metal ion solution was taken, diluted by a corresponding multiple, and the concentration of the aqueous phase was tested with an atomic absorption spectrophotometer (AA-6680) to calculate the corresponding extraction rate.

[0090] The results are as follows Figure 3 As shown, Figure 3 (a) shows the effect of HCl concentration on the extraction of Au(III). Figure 3 (b) shows the effect of HCl concentration on the extraction of Pd(II). Figure 3 The experimental conditions were: molar concentration of the extractant = 2 mmol / L, [Au(III)] = 1 mmol / L, [Pd(II)] = 2 mmol / L, and extraction time t = 6 h. Figure 3 (a) shows that at a hydrochloric acid concentration of 0.1 mol / L, both SS-C2 and SS-C5 exhibited excellent extraction effects on Au(III) (~92%), and as the hydrochloric acid concentration increased, the extraction rates of Au(III) decreased to 41.06% and 48.07%, respectively, at a hydrochloric acid concentration of 2 mol / L, and then the decrease in extraction rate decreased with the increase in hydrochloric acid concentration (~5% and ~3%). Figure 3As shown in (b), the increase in hydrochloric acid concentration is also not conducive to the extraction of Pd(II), causing the extraction rates of Pd(II) of SS-C2 and SS-C5 to gradually decrease from 93.1% and 95.9% to 64.9 and 67.1%, respectively.

[0091] Comparing the extraction results of SS-C2 and SS-C5, it was found that the extraction rates of Pd(II) were different, which may be attributed to the influence of the functional atoms and structure of the extractant. The extraction of Pd(II) depends on the coordination of sulfur atoms. Due to the interatomic spacing, the extraction of sulfur atoms is not affected by the length of the ester alkyl chain. The results show that high hydrochloric acid concentration is not conducive to the extraction of the two precious metals by the extractant, so the subsequent experiments were carried out at a hydrochloric acid concentration of 0.1 mol / L.

[0092] (3) Extraction kinetics

[0093] Extraction kinetics greatly affects the efficiency and cost of extraction in industrial applications. The present invention investigates the extraction kinetics of Au(III) and Pd(II) by extractants. Figure 4 As shown, Figure 4 (a) is the extraction kinetics result of Au(III), Figure 4 (b) in the figure shows the extraction kinetics of Pd(II). Figure 4 Experimental conditions: molar concentration of extractant = 2mmol / L, [Au(III)] = [Pd(II)] = 1mmol / L, [HCl] = 0.1mol / L, equal volumes of organic phase and aqueous phase. During the extraction of Au(III) and Pd(II), the extraction kinetics of Au(III) was slow, with SS-C2 reaching an extraction rate of 94% in 30min, while SS-C5 required 2h. The extraction kinetics of Pd(II) was extremely fast, with SS-C2 reaching equilibrium within 15min, but the extraction rate was 89%; SS-C5 reached extraction equilibrium in 30min, at which time the extraction rate was 99%. SS-C5 requires a longer equilibrium time probably because it has a stronger extraction ability for Pd(II) and a larger extraction amount of Pd(II).

[0094] The shorter the aliphatic side chain, the greater the extraction rate of Au(III). In the extraction process of Au(III), oxygen atoms participate in the coordination. The extension of the ester alkyl chain causes the electron cloud density of the ester functional group to increase, which is not conducive to the extraction of Au(III). Pd(II) mainly coordinates with sulfur atoms, and the extension of the carbon chain has no effect on the extraction of Pd(II). Therefore, extractants with short carbon chains have faster extraction rates for Au(III) and Pd(II).

[0095] (4) Extractant saturation capacity

[0096] In order to explore the extraction capacity of the extractant, the present invention sets different initial concentrations of Au(III) and Pd(II) to explore the saturated extraction capacity of the extractant. The initial concentrations of the aqueous phase are 0.25-7 mmol / L Au(III) and 0.5-6 mmol / L Pd(II), respectively. 1,2-dichloroethane containing 1 mmol / L of the extractant is used as the organic phase for extraction at 25°C for 4 hours. The results are shown in Figure 2. Figure 5 As shown, Figure 5 (a) is the extraction capacity of the extractant for Au(III) extraction, Figure 5 (b) in the figure is the extraction capacity of the extractant for Pd(II). Figure 5 The experimental conditions are as follows: the molar concentration of the extractant = 2mmol / L, [Au(III)] = 0.25-7mmol / L, [Pd(II)] = 0.5-6mmol / L, [HCl] = 0.1mol / L, and the volumes of the organic phase and the aqueous phase are equal. As the concentrations of Au(III) and Pd(II) in the aqueous phase increase, the amount of the extractant continues to increase and tends to equilibrium, indicating that the extractant has reached extraction saturation. At this time, the saturated extraction capacities of SS-C2 and SS-C5 for Au(III) are 750.60mg / g and 557.98mg / g, respectively; the saturated extraction capacities for Pd(II) are 500.17mg / g and 484.87mg / g, respectively.

[0097] The extension of the ester alkyl chain in the extractant brings steric hindrance, hindering the coordination of the "C=O" functional group in the solution with Au(III), resulting in a decrease in the extraction capacity. In the extraction process of palladium, the sulfur atom mainly participates in the coordination of palladium, so it is not affected by the extension of the ester alkyl chain. The decrease in saturation capacity can be attributed to the increase in the molecular weight of the extractant.

[0098] (5) Extraction mechanism study

[0099] The molar ratio of the extractant to the complex formed by Au(III) and Pd(II) was determined by Job's continuous variable method. The concentration of the extractant in the organic phase and the concentration of Au(III) and Pd(II) in the aqueous phase were always kept at 1mmol / L. The total volume of the organic phase and the aqueous phase was fixed at 10mL. The ratio of the two phases was changed in turn. After 4h of extraction, the organic phase and the aqueous phase were separated, and the concentrations of Au(III) and Pd(II) in the aqueous phase were detected by AAS. The results are shown in Figure 2. Figure 6 As shown, Figure 6 (a) is the Job's diagram of the extractant-Au(III) complex. Figure 6 (b) is the Job's diagram of the extractant Pd(II) complex. Figure 6The experimental conditions of (a) and (b) are: molar concentration of the extractant = 1 mmol / L, [Au(III)] = [Pd(II)] = 1 mmol / L, V O+A =10mL, volume ratio of O (organic phase) / A (aqueous phase) = 1:9 to 9:1;

[0100] The fitting lines of SS-C2 and SS-C5 reach maximum values ​​at 0.53 and 0.57, respectively. At this maximum molar ratio, the amount of Au(III) ions transferred from the aqueous phase to the organic phase is the largest. At this time, the molar ratios of the extractant to Au(III) are 1.15:1 and 1.32:1, respectively, which means that one extractant molecule coordinates with one Au(III) during the extraction process. The extension of the carbon chain is not conducive to the extraction of gold, which increases the complexation ratio of the extractant. Figure 6 As shown in (b), the molar fractions of SS-C2 and SS-C5 reach maximum values ​​at 0.43 and 0.47, when the ratios of the extractant to Pd(II) are 0.75:1 and 0.87:1, respectively. This means that the ratio of SS-C2 to Pd(II) is 3:4, which can be explained as follows: There are multiple complexing sites in the extractant result, including two sulfur atoms and two ester groups. The previously reported PdCl2-L crystal complex shows that the two sulfur atoms in the compound are directly coordinated to Pd(II). Therefore, the stronger coordination ability of SS-C2 may be due to its two sulfur atoms (i.e., chelation), and the thioether atom is bonded to the metal center in a bidentate mode. At the same time, due to the presence of the ester group, the C=O of the ester group has a weak interaction with Pd(II). Compared with the coordination ratio of dithiodiethanolamide to Pd(II) (1:1), SS-C2 and SS-C5 exhibit stronger coordination ability and are more suitable extractants for extracting Pd(II).

[0101] The extraction equation of Au(III) is shown in Equation 4:

[0102]

[0103] The extraction equation of Pd(II) is shown in Equation 5:

[0104]

[0105] HCl is known to have a negative impact on the extraction of metal ions, so the extraction of H + and Cl - Effects on the extraction of Au(III) and Pd(II). First, Cl - The concentration of H + The concentration of H +The concentration of Cl is 0.1 mol / L. - The concentration varies in the range of 0.1 to 4 mol / L. + and Cl - Effect of concentration on the extraction of Au(III) Figure 7 As shown in (a) and (b) in . Figure 7 (a) in the equation is H + Effect of concentration on the extraction of Au(III), Figure 7 (b) in the equation is Cl - Effect of concentration on the extraction of Au(III); Figure 7 (c) in the equation is H + Effect of concentration on the extraction of Pd(II), Figure 7 (d) in the equation is Cl - Effect of concentration on the extraction of Pd(II). Figure 7 The experimental conditions of (a) to (d) are as follows: molar concentration of the extractant = 2 mmol / L, [Au(III)] = 1 mmol / L, [Pd(II)] = 2 mmol / L, extraction time t = 4 h, and the organic phase and the aqueous phase have equal volumes.

[0106] Follow H + With the increase of concentration, the extraction rate of Au(III) by SS-C2 and SS-C5 decreased, indicating that the extraction of Au(III) was affected by H + The influence of Cl concentration. - With the increase of concentration, the extraction of Au(III) first decreased rapidly and then decreased slowly, and the downward trend was consistent with the effect of HCl. - The negative effect of concentration is mainly due to Cl - With AuCl4 - The competitive relationship between + The influence of and Cl- on the extraction efficiency of Pd(II) is different from that of Au(III), e.g. Figure 7 (c) and (d) in H + The extraction rate of Pd(II) remained almost unchanged with the increase of Cl - The increase of makes the extraction rate of Pd(II) decrease, indicating that the extraction process of Pd(II) is mainly affected by Cl-. In the concentration range of 0.1~4mol / L hydrochloric acid, the main form of Pd(II) is PdCl4 2- When the Cl- concentration in the solution is high, PdCl4 2- It will compete strongly with excess Cl- and is not conducive to extraction.

[0107] The UV-Vis characterization method was used to detect the ultraviolet absorption wavelength of the extracted complex. Figure 8 As shown, Figure 8 (a) is the ultraviolet absorption peak of SS-C2 and gold and palladium complexes. Figure 8 (b) in the figure is the ultraviolet absorption peak of SS-C5 complex with gold and palladium.

[0108] The maximum absorption wavelength of the extractant SS-C2 is 225.5nm, and the metal ions Au(III) and Pd(II) show an absorption peak near 225nm after complexing with the extractant, and there is no absorption peak at AuCl4 - (313, 227nm) and PdCl4 2- The corresponding peaks of (280, 222nm) indicate that the chloride form of metal ions in the extraction complex has changed. + Concentration and Cl - The concentration experimental results show that the structures of the extractants are AuCl3·nL and PdCl2·nL, which are consistent with the above experimental inference. The extractants SS-C5 and SS-C2 have the same structure, and the UV results are the same as above.

[0109] (6) Ion selectivity

[0110] Selective extraction of Au(III) and Pd(II) has important practical application significance. At the same time, hydrochloric acid concentration is also one of the factors affecting extraction separation. Therefore, the present invention prepares a mixed metal ion solution composed of 1mmol / L Au(III), Pd(II), Cu(II), Fe(III), Ni(II), Co(II), Pb(II) and Zn(II), and tests the extraction of precious metal ions by the extractant at 0.1mol / L, 1.0mol / L and 3.0mol / L hydrochloric acid concentrations. Fig. 9 (a) is the extraction efficiency of SS-C2 for simulated mixed metal ion solution. Fig. 9 (b) is the extraction efficiency of SS-C5 for simulated mixed metal ion solution. Fig. 9 The experimental conditions of (a) and (b) are as follows: the molar concentration of the extractant = 2 mmol / L, the molar concentration of the above-mentioned metal ions = 1 mmol / L, [HCl] = 0.1-3 mol / L, O / A = 1 (equal volumes of organic phase and aqueous phase), extraction temperature of 25°C, and extraction time of 4 h. Fig. 9 (c) in the figure is the extraction of mixed metal ion solution by 4 mmol / L extractant.

[0111] Fig. 9(a) and (b) in the figure show the extraction results of metal ions by extractants SS-C2 and SS-C5 at different hydrochloric acid concentrations. When the concentration of aqueous hydrochloric acid was 0.1 mol / L, the extraction rates of Au(III) and Pd(II) in the mixed solution by SS-C2 were 91.9% and 87.6%, respectively, and the extraction rates of Cu(II), Fe(III), Ni(II), Co(II), Pb(II) and Zn(II) were 3.7%, 3.1%, 0%, 0.6%, 1.4% and 0%, respectively, all lower than 4%. Therefore, the extraction of other coexisting metal ions can be ignored. As the concentration of HCl increases, the extraction trend of Au(III) and Pd(II) is consistent with the effect of hydrochloric acid concentration on the experiment, that is, the extraction rate decreases at high acidity. Except for the extraction rate of Zn(II), which increases with the increase of hydrochloric acid concentration to 5.1%, the extraction rates of other base metal ions are all lower than 5%. The extraction results of mixed metal ions by extractant SS-C5 are the same as those of extractant SS-C2, that is, the best extraction effect for Au(III) and Pd(II) is achieved at a concentration of 0.1 mol / L HCl, reaching 66.5% and 98.9%, and the extraction rate of impurity ions is less than 6%. Increasing the concentration of hydrochloric acid, the extraction rate of gold by SS-C5 decreases. However, the extraction rate of palladium remains above 95%, which shows that SS-C5 has excellent selectivity for palladium, excellent resistance to impurity ion interference and acid resistance, and a wide range of acidity adaptability.

[0112] During the extraction process, SS-C5 found that the gold extraction rate was only 66.5%. Therefore, the concentration of the extractant was increased to further explore the selectivity of the extractant. The results are as follows Fig. 9 As shown in (c) in the figure. As the concentration of the extractant increased, the extraction rate of gold reached 95-99%, the extraction rate of palladium was above 99%, and the extraction rates of other metal ions did not increase with the increase in the amount of extractant used. Therefore, these results show that SS-C2 and SS-C5 have good selectivity for Au(III) and Pd(II) and are not affected by other metal ions. This also shows that the extractant has great potential for separating Au(III) and Pd(II) from actual mixed metal ions.

[0113] (7) Reusability

[0114] The stripping experiment used SS-C5 as an experimental model to explore its reusability. The stripping effects of 1 mol / L oxalic acid, ammonia water and thiourea on Au(III) and Pd(II) were investigated.

[0115] The specific experimental process is as follows: prepare 4 centrifuge tubes for the stripping experiment, separate the aqueous phase and the organic phase after the extraction, add different stripping agents (5mL, the volume ratio of stripping agent to metal-loaded organic phase is 1:1) to the metal-loaded organic phase (5mL), and stripping is performed at 25°C and 230rpm. After the stripping is completed, the concentration of metal ions in the aqueous phase is detected by AAS, and the organic phase enters the next extraction-stripping cycle after washing with water.

[0116] The results are shown in Table 2. The stripping results show that thiourea has the highest stripping rate, which can reach 92.4% and 61.2%. After changing the acidity of the thiourea solution, the stripping rate of Au(III) and Pd(II) can reach 100%, because the acidic thiourea solution is a stripping agent with faster kinetics, which can form cationic metal-thiourea complexes. The stripping process includes the reduction of Au(III) to Au(I) by thiourea compounds, followed by the formation of Au(I)-thiourea complex Au(CS(NH2)2) 2+ In acidic thiourea solution, palladium is stripped to form PdCl2·(NH2)2CS, which can be attributed to the fact that the S atoms in thiourea prefer to bind to the soft metal palladium. The good stripping rate of acidic thiourea for Au(III) and Pd(II) indicates that the material is reusable.

[0117] Table 2 Stripping effect of different stripping agents

[0118] Serial number Stripping reagent <![CDATA[S Au(III) %(SS-C5)]]> <![CDATA[S Pd(II) %(SS-C5)]]> 1 1mol / L oxalic acid 0.0 1.9 2 1mol / L ammonia water 32.9 30.8 3 1mol / L thiourea 92.4 61.2 4 0.5mol / L thiourea + 1mol / L HCl 100.0 100.0

[0119] It can be seen from the above examples that the present invention successfully prepared the extractants 1,2-(carboxyethylmethylthio)-ethane (SS-C2) and 1,2-bis(carboxypentylmethylthio)-ethane (SS-C5), and dissolved them in 1,2-dichloroethane for efficient and selective recovery of Au(III) and Pd(II) from aqueous solution.

[0120] The present invention determines the optimal extraction experimental conditions: using 1,2-dichloroethane as a diluent, under 0.1 mol / L HCl, 2 mmol / L of extractant extracts 1 mmol / L of metal ions, the equilibrium time required for extracting gold is 2 hours, and the equilibrium time required for extracting palladium is 30 minutes.

[0121] Under the optimal experimental conditions, the extractants provided by the present invention have saturated capacities of SS-C2 and SS-C5 for extracting Au(III) of 750.60 mg / g and 557.98 mg / g, respectively, and saturated capacities of SS-C2 and SS-C5 for extracting Pd(II) of 500.17 mg / g and 484.87 mg / g, respectively.

[0122] The present invention determines that the complexation ratio of the extractant to Au(III) is 1:1 and the complexation ratio to Pd(II) is 3:4 by Job's method. Combining experiments and instrument characterization, it is proposed that the extraction mechanism of the extractant for Au(III) is a solvation mechanism, and the extraction mechanism of Pd(II) is a coordination substitution mechanism.

[0123] The present invention has found through the study of selectivity experiments that the extractant has high selectivity and high extraction rate for Au(III) and Pd(II) under low acidity, and increasing the concentration of the extractant will increase the extraction rate for Au(III) and Pd(II) without extracting metal impurity ions, indicating that the extractant has excellent selectivity.

[0124] The invention proves that the extractant has the property of repeated utilization through the stripping of the acidic thiourea solution.

[0125] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A disulfide compound, It is characterized in that It has the structure shown in formula 1: In formula 1: R is a C1-10 alkyl group.

2. The disulfide compound according to claim 1, It is characterized in that R is ethyl or n-pentyl.

3. The method for preparing the disulfide compound according to claim 1 or 2, It is characterized in that The following steps are involved: Mixing 1,2-bis(carboxymethylthio)-ethane, thionyl chloride and an organic solvent to carry out an acyl chloride reaction to obtain an acyl chloride product; The acyl chloride product has a structure shown in Formula 2: The acyl chloride product, organic base and alkyl alcohol are mixed for substitution reaction to obtain a disulfide compound with a structure shown in Formula 1; the alkyl alcohol has a structure shown in Formula 3: R-OH Formula 3.

4. Use of the disulfide compound according to claim 1 or 2 or the disulfide compound prepared by the preparation method according to claim 3 in recovering precious metals by solvent extraction.

5. The use according to claim 4, It is characterized in that The noble metal includes gold and / or palladium.

6. A method for recovering precious metals by solvent extraction, It is characterized in that The following steps are involved: The extractant organic phase solution and the aqueous phase solution containing precious metals are mixed for extraction to obtain an extracted organic phase enriched with precious metals and a raffinate aqueous phase; the extractant organic phase solution comprises an extractant and an organic diluent, and the extractant is the disulfide compound according to claim 1 or 2 or the disulfide compound prepared by the preparation method according to claim 3; the aqueous phase solution containing precious metals is an acidic solution.

7. The method according to claim 6, It is characterized in that The organic diluent includes one or more of kerosene, n-hexane, toluene, xylene, chloroalkane and butyl acetate; The molar concentration of the extractant in the extractant organic phase solution is 2 mmol / L.

8. The method according to claim 6, It is characterized in that The aqueous solution containing precious metals comprises precious metals, water and inorganic strong acid; in the aqueous solution containing precious metals: the molar concentration of the precious metals is 0.25-7 mmol / L, and the molar concentration of the inorganic strong acid is 0.1-4 mol / L.

9. The method according to any one of claims 6 to 8, It is characterized in that The volume ratio of the organic phase solution of the extractant to the aqueous phase solution containing precious metals is 1:9 to 9:1; the extraction temperature is room temperature, and the extraction time is ≥15 minutes.

10. The method according to claim 6, It is characterized in that After obtaining the extracted organic phase enriched in precious metals, the method further comprises: mixing the extracted organic phase enriched in precious metals with a stripping agent aqueous phase solution for stripping to obtain an extracted aqueous phase enriched in precious metals and a raffinate organic phase; the stripping agent aqueous phase solution comprises a stripping agent and water, and the stripping agent comprises oxalic acid, NH 3 Or thiourea, or the stripping agent is a mixture of thiourea and HCl.