Modified hydroxypropyl methyl cellulose as well as preparation method and application thereof in mortar
By increasing the methoxy group substitution degree of hydroxypropyl methylcellulose and grafting organic matter, it forms modified hydroxypropyl methylcellulose, which solves the insufficient anti-mold and mechanical properties of its mildew in a humid environment. The problem has achieved the efficient hydrophobicity and mechanical performance improvement of the mortar.
Patent Information
- Application Number
- CN202410972919.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
The existing hydroxypropyl methylcellulose has poor anti-mold properties in mortar and is difficult to use in humid environments for a long time. The traditional methods affect the hydrophobicity and mechanical properties of the mortar.
By increasing the methoxy group substitution degree of hydroxypropyl methylcellulose and forming modified hydroxypropyl methylcellulose by grafting organic matter, it enhances its bonding, hydrophobicity and mechanical properties, combining vinyl three (2-methoxyethoxy)silane, allyl carbamate and polyvinyl alcohol react to form a crosslinked structure to improve performance.
It significantly improves the bonding performance, hydrophobic properties, mildew resistance and mechanical properties of the mortar, making it possible to be used for a long time in a humid environment, and enhances compressive strength, crack resistance and stability.
Smart Images

Figure BDA0004953741070000041 
Figure BDA0004953741070000051 
Figure BDA0004953741070000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and particularly relates to modified hydroxypropyl methylcellulose and a preparation method thereof and application thereof in mortar. Background Art
[0002] Cellulose ethers are a class of versatile polymer additives that play an important role in multiple industries, including textiles, plastic manufacturing, medicine, construction, and food processing. In cement-based materials, non-ionic cellulose ethers such as methylcellulose, hydroxypropyl methylcellulose, and hydroxyethyl methylcellulose are widely used, especially hydroxypropyl methylcellulose, which can effectively improve the adhesion and water retention of concrete because the hydroxyl groups and ether bonds in its molecular structure can combine with water molecules through hydrogen bonds.
[0003] With the rapid advancement of urbanization and the development of the construction industry, the performance and quality requirements for mortar are also constantly increasing. Through continuous technological innovation and material research and development, more reliable and environmentally friendly mortar solutions can be provided for the construction industry to promote the sustainable development of the industry. Therefore, the development of new mortar additives that are environmentally friendly, efficient, and highly adaptable has become an important direction for the development of the industry.
[0004] The production of hydroxypropyl methylcellulose usually involves chemical reactions of cotton fibers in a specific solvent system, including steps such as alkalization, etherification, acid washing and neutralization. However, traditional hydroxypropyl methylcellulose contains more hydrophilic groups (hydroxyl groups and ether bonds), which affects its hydrophobicity; at the same time, it may cause the mortar surface to become too slippery, thereby affecting the bonding effect between the mortar and the substrate.
[0005] Chinese patent CN 110655345 A relates to a modified hydroxypropyl methylcellulose ether dry powder, including hydroxypropyl methylcellulose ether, polyvinyl alcohol, polyacrylamide, white carbon black, polycarboxylic acid water reducer and hydroxypropyl starch ether. The external wall insulation plastering mortar made of the modified hydroxypropyl methylcellulose ether dry material has a high water retention rate, high early strength, no powdering phenomenon, and no cracking; however, its mildew resistance is poor, which is not conducive to long-term use in humid areas or walls susceptible to moisture.
[0006] Therefore, there is an urgent need for a modified hydroxypropyl methylcellulose that can be applied to a mortar system to improve the water resistance, mildew resistance, and crack resistance of the mortar, and further improve the mechanical properties of the mortar so that it can be used for a long time in places prone to moisture. Summary of the invention
[0007] In view of the existing technical problems, the purpose of the present invention is to provide a modified hydroxypropyl methylcellulose and a preparation method thereof and an application thereof in mortar. The hydroxypropyl methylcellulose obtained by the preparation method of the modified hydroxypropyl methylcellulose of the present invention increases the degree of substitution of the methoxyl group, and then is grafted with organic matter to form modified hydroxypropyl methylcellulose, thereby improving its adhesion and hydrophobicity. The present invention further applies the prepared modified hydroxypropyl methylcellulose to mortar, which can make the mortar have good adhesion, hydrophobicity, mildew resistance and mechanical properties, and can be used for a long time in places prone to moisture.
[0008] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0009] The present invention first provides a method for preparing modified hydroxypropyl methylcellulose, comprising the following steps:
[0010] S1. Place cotton powder in a dispersed system of a mixed solvent, add sodium hydroxide, heat and react for 30-40 minutes under an inert gas atmosphere, cool to 25°C, stir and react for 1-1.5 hours to obtain alkali cellulose;
[0011] S2. Add propylene oxide and methyl chloride to the alkali cellulose obtained in step S1, heat to 55-65 ° C for 1.5-2h, and heat to 80-90 ° C for 1.5-2h to obtain a material;
[0012] S3. The material obtained in step S2 is acidified to adjust the pH to neutral, and the solvent is recovered, and then dried and crushed to obtain hydroxypropyl methylcellulose;
[0013] S4. Vinyl tri(2-methoxyethoxy)silane and deionized water were stirred and mixed, the pH value was adjusted to 2-3, heated to 40-50° C. for hydrolysis for 10-15 h, and then the hydroxypropyl methylcellulose obtained in step S3 was added and stirred to obtain silane-modified hydroxypropyl methylcellulose;
[0014] S5. Add 6-(allyloxycarbonylamino)-1-hexanol, ammonium persulfate, and solvent to a reaction kettle, heat to 75-85° C., add the silane-modified hydroxypropyl methylcellulose obtained in step S4, stir and react at a constant temperature of 75-85° C. for 3-5 hours, cool to room temperature, adjust the pH value to neutral, wash, and filter to obtain a modified hydroxypropyl methylcellulose intermediate;
[0015] S6. Add polyvinyl alcohol and deionized water to the reactor, stir and mix, add 25-35wt% hydrogen peroxide solution, stir and react for 30-40min, add the modified hydroxypropyl methylcellulose intermediate obtained in step S5, stir and react for 30-60min, dry, and grind to obtain modified hydroxypropyl methylcellulose.
[0016] In some embodiments, the cotton powder needs to be pre-processed by pulverization to make its mesh size 60-120 meshes.
[0017] In some embodiments, the mixed solvent is toluene, isopropanol and water, and the mass ratio of the three is (5-9):1:(0.5-0.9).
[0018] In some embodiments, the mass ratio of methyl chloride to cotton powder is 1:(1-1.3).
[0019] In some embodiments, the mass ratio of methyl chloride to propylene oxide is (2.1-2.5):1.
[0020] In some embodiments, the mass ratio of vinyl tris(2-methoxyethoxy)silane to hydroxypropyl methylcellulose in step S4 is 1:(2-5).
[0021] Preferably, in step S4, the mass ratio of vinyl tri(2-methoxyethoxy)silane to hydroxypropyl methylcellulose is 1:3.5.
[0022] In some embodiments, the mass ratio of 6-(allyloxycarbonylamino)-1-hexanol to silane-modified hydroxypropyl methylcellulose in step S5 is 1:(2.5-4).
[0023] Preferably, in step S5, the mass ratio of 6-(allyloxycarbonylamino)-1-hexanol to silane-modified hydroxypropyl methylcellulose is 1:3.
[0024] In some embodiments, the mass ratio of the polyvinyl alcohol, the 25-35 wt % hydrogen peroxide solution and the modified hydroxypropyl methylcellulose intermediate in step S6 is 1:(0.01-0.05):(1-2).
[0025] Preferably, in step S6, the mass ratio of the polyvinyl alcohol, the 30 wt % hydrogen peroxide solution and the modified hydroxypropyl methylcellulose intermediate is 1:0.03:1.5.
[0026] The invention adjusts the dosage of methyl chloride, propylene oxide and sodium hydroxide so as to increase the substitution degree of methoxy groups of hydroxypropyl methylcellulose, thereby changing the surface tension characteristics of hydroxypropyl methylcellulose; vinyl tris (2-methoxyethoxy) silane, allyl carbamate and polyvinyl alcohol are grafted after synthesizing hydroxypropyl methylcellulose to form modified hydroxypropyl methylcellulose, so as to improve its comprehensive performance.
[0027] The hydrolysis reaction of vinyl tri(2-methoxyethoxy)silane can generate a cross-linked polymer with a network structure. This network structure provides a dispersing medium for hydroxypropyl methylcellulose, allowing hydroxypropyl methylcellulose to be evenly distributed in it, thereby playing its role of connection and support. In addition, the hydrolyzed silanol groups react with the hydroxyl groups in hydroxypropyl methylcellulose to form a cross-linked structure of siloxane bridges (Si-O-Si). This cross-linking enhances the water resistance, compressive strength, crack resistance and other properties of hydroxypropyl methylcellulose.
[0028] 6-(allyloxycarbonylamino)-1-hexanol can be grafted through the addition reaction between olefins, and the carbamate group makes hydroxypropyl methylcellulose have better bonding properties and stronger hydrophobicity, thereby making it perform better in a humid environment.
[0029] The applicant grafted polyvinyl alcohol onto hydroxypropyl methylcellulose to make it have better water retention, crack resistance, durability, impermeability and adhesion. Polyvinyl alcohol is dissolved in water to form a uniform solution. After adding 30wt% hydrogen peroxide solution, the hydroxyl groups in the polyvinyl alcohol are oxidized to form aldehyde groups, and then the hydroxyl groups on the hydroxypropyl methylcellulose and 6-(allyloxycarbonylamino)-1-hexanol react with the aldehyde groups to form a cross-linked structure, which effectively enhances the mechanical properties and stability of the hydroxypropyl methylcellulose. At the same time, the generated Schiff base group (-CH=N-) further enhances its hydrophobicity.
[0030] The present invention secondly provides a modified hydroxypropyl methylcellulose prepared by the preparation method.
[0031] The third aspect of the present invention provides a modified hydroxypropyl methylcellulose prepared by the preparation method or the use of the modified hydroxypropyl methylcellulose in mortar, wherein the mortar comprises the following raw materials in parts by weight:
[0032]
[0033] In some embodiments, the method for preparing the mortar comprises the following steps:
[0034] 1. Mix cement, yellow sand, fly ash and vitrified microspheres evenly and stir to obtain premix 1;
[0035] 2. adding modified hydroxypropyl methylcellulose, surfactant and polypropylene fiber to the above premix and stirring to obtain premix 2;
[0036] 3. Add the premix 1 obtained in step 1 to the premix 2 obtained in step 2, then add the mildew-proofing and fungicide, water-reducing agent and defoaming agent to mix, and then put into the dry mixing equipment to obtain mortar.
[0037] In some embodiments, the polypropylene fibers have a length of 5-15 mm.
[0038] In some embodiments, the surfactant is nonylphenol polyoxyethylene ether.
[0039] Preferably, the nonylphenol polyoxyethylene ether is OP-9 or OP-10.
[0040] In some embodiments, the method for preparing the mildew and fungicide comprises the following steps:
[0041] (1) adding 5-chloro-isothiazoline-3-one, maleic anhydride and xylene into a reaction kettle, heating to 115-125° C. under an inert gas atmosphere, keeping the temperature for reaction for 7-8 hours, washing and drying to obtain a reactant;
[0042] (2) Add the reactant obtained in step (1), ethyl para-aminobenzenesulfonate, N,N-dimethylformamide and ethanol to a reaction kettle, then add a carbodiimide condensation agent and an activator, stir, and react for 5-6 hours to obtain a mildew and fungicide.
[0043] In some embodiments, the molar ratio of 5-chloro-isothiazoline-3-one to maleic anhydride in step (1) is 1:(1.1-1.4).
[0044] In some embodiments, the molar ratio of the reactant to ethyl para-aminobenzenesulfonate in step (2) is 1:(1.1-1.4).
[0045] In some embodiments, the antifungal fungicide has the following structural formula:
[0046]
[0047] Preferably, the molar ratio of 5-chloro-isothiazoline-3-one to maleic anhydride in step (1) is 1:1.2.
[0048] In some embodiments, the cement is Portland cement.
[0049] In some embodiments, the defoaming agent is a silicone defoaming agent.
[0050] In some embodiments, the water reducer is a polycarboxylate water reducer.
[0051] On the other hand, the reaction mechanism and effect of the present invention are as follows:
[0052] 1. The sticky properties of hydroxypropyl methylcellulose itself can increase the bonding force in the mortar. When the mortar is mixed with water, this sticky effect helps to improve the overall bonding performance of the mortar to enhance its construction performance; at the same time, the modified hydroxypropyl methylcellulose further improves the hydrophobicity, compressive strength, crack resistance and bonding performance of the mortar.
[0053] 2.5-Chloro-isothiazoline-3-one is a broad-spectrum bactericidal preservative with good sterilization effects on most bacteria, molds and yeasts, especially its ability to inhibit bacteria is significantly better than fungi. It can effectively kill a variety of bacteria at extremely low concentrations with high sterilization efficiency. The formation of calcium hydroxide during cement hydration makes the mortar system alkaline, and this alkaline environment is crucial to ensure the performance and durability of the mortar.
[0054] However, 5-chloro-isothiazoline-3-one will be partially inactivated under alkaline conditions. The applicant introduced maleic anhydride through N substitution to graft carboxyl groups on the molecular structure of 5-chloro-isothiazoline-3-one, and then reacted with methyl p-aminobenzenesulfonate to form an antifungal fungicide, which can maintain its activity in the mortar system and effectively inhibit bacteria and mildew. In addition, the introduced double bonds and benzene rings can effectively improve the hydrophobicity of the mortar and broaden its use in humid environments.
[0055] 3. The polypropylene fiber of the present invention significantly improves the mechanical properties of the mortar, effectively reduces the shrinkage force and shape change of cement during the early drying process, and prevents the formation of cracks due to stress concentration during the hardening process; in addition, the applicant's preferred length of polypropylene fiber helps to enhance the fluidity of the mortar. At the same time, when used in combination with modified hydroxypropyl methylcellulose, it can further increase the air content in the mortar, thereby improving the durability of the mortar, enhancing the anti-seepage performance, and reducing water seepage and sedimentation.
[0056] Compared with the prior art, the present invention has the following beneficial effects:
[0057] 1. The modified hydroxypropyl methylcellulose of the present invention has better adhesion and hydrophobicity. In the mortar system, the modified hydroxypropyl methylcellulose effectively enhances the water resistance, compressive strength, crack resistance, adhesion and stability of the mortar; at the same time, the mildew-proofing and fungicide effectively enhances the hydrophobicity and antibacterial and mildew-proof properties of the mortar.
[0058] 2. The hydroxypropyl methylcellulose prepared by the present invention increases the degree of substitution of the methoxy group, thereby changing the surface tension characteristics of the hydroxypropyl methylcellulose.
[0059] After synthesizing hydroxypropyl methylcellulose, vinyl tri(2-methoxyethoxy) silane, allyl carbamate, and polyvinyl alcohol are grafted to form modified hydroxypropyl methylcellulose to improve its comprehensive performance. First, the use of vinyl tri(2-methoxyethoxy) silane to form a siloxane-bridged cross-linked structure enhances the water resistance, compressive strength, crack resistance and other properties of hydroxypropyl methylcellulose; second, the introduction of carbamate groups gives hydroxypropyl methylcellulose better adhesion and hydrophobicity; third, the applicant grafts polyvinyl alcohol onto hydroxypropyl methylcellulose to give it better water retention, crack resistance, durability, impermeability and adhesion. In addition, the cross-linked structure formed by the Schiff base reaction effectively enhances the mechanical properties, stability and hydrophobicity of hydroxypropyl methylcellulose.
[0060] 3. The present invention forms a mildew-proofing and fungicide by modifying 5-chloro-isothiazoline-3-one, so that it can maintain activity in the alkaline environment of mortar, thereby effectively inhibiting bacteria and preventing mildew. In addition, the introduced double bonds and benzene rings can effectively improve the hydrophobicity of the mortar and broaden its use in humid environments. DETAILED DESCRIPTION
[0061] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, rather than to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0062] Each mortar was prepared according to the proportions of the raw materials and the preparation methods specified in the following examples and comparative examples.
[0063] In order to facilitate those skilled in the art to implement the present invention, some raw material manufacturers of the embodiments and comparative examples are described as follows:
[0064] Nonylphenol polyoxyethylene ether: purchased from nonylphenol polyoxyethylene ether, model OP-10;
[0065] Polycarboxylate water reducer: purchased from Shandong Maofa Chemical Co., Ltd., with an active ingredient content of 99%;
[0066] Polypropylene fiber: purchased from Shandong Hongju Engineering Materials Co., Ltd., 9 mm;
[0067] Silicone defoamer: purchased from Shanghai Ziyi Chemical Co., Ltd., model ZY-1024;
[0068] Hydroxypropyl methylcellulose: purchased from Shijiazhuang Xinweite Building Materials Co., Ltd.;
[0069] Polyvinyl alcohol: purchased from Henan Youchuang Chemical Products Co., Ltd.
[0070] Portland cement: purchased from Aohong Mineral Products Business Department, Lingshou County;
[0071] Yellow sand: purchased from Shanghai Dacheng Building Materials Co., Ltd.;
[0072] Fly ash: purchased from Hebei Chuangtian Engineering Materials Co., Ltd., mesh size 325;
[0073] Vitrified microspheres: purchased from Puyang Changshun Insulation Technology Co., Ltd., mesh size 200.
[0074] Other raw materials are not specially specified and can be purchased from the market.
[0075] Preparation Example 1
[0076] The preparation method of modified hydroxypropyl methylcellulose A comprises the following steps:
[0077] S1. 3.5 kg of 100-mesh cotton powder was placed in a dispersion system of 25 kg of toluene, 3.5 kg of isopropanol, and 0.5 kg of methanol, and then 4 kg of sodium hydroxide and 2.5 kg of water were added. Under a nitrogen atmosphere, the mixture was heated for 35 min, cooled to 25 ° C, and stirred for 1 h to obtain alkali cellulose;
[0078] S2. Add 1.75 kg propylene oxide and 3.85 kg methyl chloride to the alkali cellulose obtained in step S1, heat to 60 ° C for 2 h, and heat to 85 ° C for 2 h to obtain a material;
[0079] S3. The material obtained in step S2 was adjusted to pH 7 with 0.5 mol / L hydrochloric acid, and the solvent was recovered, and then dried at 105°C and crushed to obtain hydroxypropyl methylcellulose;
[0080] S4. 0.5 kg of vinyl tris (2-methoxyethoxy) silane and 500 ml of deionized water were stirred and mixed, 1 mol / L hydrochloric acid was added to adjust the pH value to 3, heated to 45 ° C for hydrolysis for 12 h, and then 1.75 kg of hydroxypropyl methylcellulose obtained in step S3 was added and stirred for 1 h to obtain silane-modified hydroxypropyl methylcellulose;
[0081] S5. 0.75 kg of allyl carbamate, 60 g of ammonium persulfate, and 4.5 kg of acetone were added to a reactor, heated to 80 ° C, 2.25 kg of silane-modified hydroxypropyl methylcellulose obtained in step S4 was added dropwise, and the reaction was stirred at a constant temperature of 80 ° C for 3-5 h, cooled to room temperature, adjusted the pH value to neutral, washed with acetone 3 times, and filtered to obtain a modified hydroxypropyl methylcellulose intermediate;
[0082] S6. Add 1 kg of polyvinyl alcohol and 5 kg of deionized water to the reactor, stir and mix, add 30 g of 30 wt % hydrogen peroxide solution, stir and react for 30-40 min, add 1.5 kg of the modified hydroxypropyl methylcellulose intermediate obtained in step S5, stir and react for 30-60 min, dry at 105 ° C for 8 h, and grind to obtain modified hydroxypropyl methylcellulose A.
[0083] Preparation Example 2
[0084] The preparation method of modified hydroxypropyl methylcellulose B comprises the following steps:
[0085] S1. 3.5 kg of 100-mesh cotton powder was placed in a dispersion system of 25 kg of toluene, 3.5 kg of isopropanol, and 0.5 kg of methanol, and then 4 kg of sodium hydroxide and 2.5 kg of water were added. Under a nitrogen atmosphere, the mixture was heated for 35 min, cooled to 25 ° C, and stirred for 1 h to obtain alkali cellulose;
[0086] S2. Add 1.75 kg propylene oxide and 3.85 kg methyl chloride to the alkali cellulose obtained in step S1, heat to 60 ° C for 2 h, and heat to 85 ° C for 2 h to obtain a material;
[0087] S3. The material obtained in step S2 was adjusted to pH 7 with 0.5 mol / L hydrochloric acid, and the solvent was recovered, and then dried at 105°C and crushed to obtain hydroxypropyl methylcellulose;
[0088] S4. 0.5 kg of vinyl tri(2-methoxyethoxy)silane and 500 ml of deionized water were stirred and mixed, 1 mol / L hydrochloric acid was added to adjust the pH value to 3, heated to 45° C. for hydrolysis for 12 h, and then 1.75 kg of hydroxypropyl methylcellulose obtained in step S3 was added, stirred for 1 h, and dried at 105° C. for 6 h to obtain modified hydroxypropyl methylcellulose B.
[0089] Preparation Example 3
[0090] The preparation method of modified hydroxypropyl methylcellulose C is the same as that of Preparation Example 1, except that 0.5 kg of hydroxypropyl methylcellulose obtained in Step S3 is added in Step S4.
[0091] Preparation Example 4
[0092] The preparation method of mildew-proofing and fungicide A comprises the following steps:
[0093] (1) 0.1 mol of 5-chloro-isothiazoline-3-one, 0.12 mol of maleic anhydride, and 180 ml of xylene were added to a reaction kettle, heated to 120° C. under a nitrogen atmosphere, kept warm for 8 hours, washed twice with xylene, and dried at 150° C. for 24 hours to obtain a reactant;
[0094] (2) 0.15 mol of the reactant obtained in step (1), 0.18 mol of ethyl p-aminobenzenesulfonate, 200 ml of N,N-dimethylformamide and 80 ml of ethanol were added to a reaction kettle, and then 50 mmol of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 30 mmol of N-hydroxysuccinimide were added, and the mixture was stirred for reaction for 5 hours to obtain antifungal and fungicide A.
[0095] Preparation Example 5
[0096] The preparation method of mildew-proofing and fungicide B is the same as that of Preparation Example 4, except that the amount of maleic anhydride added is 0.2 mol.
[0097] Example 1
[0098] Application of modified hydroxypropyl methylcellulose in mortar, wherein the mortar comprises the following raw materials in parts by weight:
[0099]
[0100] The preparation method of the mortar in this embodiment comprises the following steps:
[0101] 1. Mix the silicate cement, yellow sand, fly ash and vitrified microspheres evenly, and stir at 1600 r / min for 20 min to obtain premix 1;
[0102] 2. Add modified hydroxypropyl methylcellulose A, nonylphenol polyoxyethylene ether OP-10 and polypropylene fiber to the above premix, and stir at 1600 r / min for 15 min to obtain premix 2;
[0103] 3. Add the premix 1 obtained in step 1 to the premix 2 obtained in step 2, then add the mildew-proofing and fungicide A, polycarboxylic acid water-reducing agent and silicone defoaming agent ZY-1024 to mix, and then put into the dry mixing equipment to obtain mortar.
[0104] Example 2
[0105] Application of modified hydroxypropyl methylcellulose in mortar, wherein the mortar comprises the following raw materials in parts by weight:
[0106]
[0107]
[0108] The preparation method of the mortar in this embodiment is the same as that in Example 1.
[0109] Example 3
[0110] Application of modified hydroxypropyl methylcellulose in mortar, wherein the mortar comprises the following raw materials in parts by weight:
[0111]
[0112] The preparation method of the mortar in this embodiment is the same as that in Example 1.
[0113] Example 4
[0114] A modified hydroxypropyl methylcellulose is used in mortar. The specific implementation method is the same as that of Example 1, except that an equal amount of modified hydroxypropyl methylcellulose B is used to replace the modified hydroxypropyl methylcellulose A.
[0115] Example 5
[0116] A modified hydroxypropyl methylcellulose is used in mortar. The specific implementation method is the same as that of Example 1, except that an equal amount of modified hydroxypropyl methylcellulose C is used to replace the modified hydroxypropyl methylcellulose A.
[0117] Example 6
[0118] A modified hydroxypropyl methylcellulose is used in mortar. The specific implementation method is the same as that of Example 1, except that an equal amount of antifungal agent B is used to replace antifungal agent A.
[0119] Example 7
[0120] A modified hydroxypropyl methylcellulose is used in mortar. The specific implementation method is the same as that of Example 1, except that an equal amount of commercially available 5-chloro-isothiazoline-3-one is used to replace the mildew and fungicide A.
[0121] Comparative Example 1
[0122] A modified hydroxypropyl methylcellulose is used in mortar. The specific implementation method is the same as that of Example 1, except that an equal amount of commercially available hydroxypropyl methylcellulose is used to replace the modified hydroxypropyl methylcellulose A.
[0123] Effect evaluation:
[0124] The mortars prepared in the above-mentioned Examples 1-7 and Comparative Example 1 were tested and analyzed, and the specific results are shown in Table 1.
[0125] Performance Test:
[0126] (1) Contact angle test:
[0127] The contact angle between the mortars prepared in the examples and comparative examples and water was measured using a contact angle meter. The contact angle refers to the angle between the solid-liquid interface through the liquid interior to the gas-liquid interface at the interface between the solid, liquid and gas phases. The larger the angle, the stronger the hydrophobicity.
[0128] (2) 28-day compressive strength test:
[0129] Fill the compressive strength test mold with mortar. After the mortar is left to harden for 28 days, the pressure required to fract the test block with a compression machine divided by the compressed area of the test block is the compressive strength value of the mortar.
[0130] (3) Anti-mildew test:
[0131] The anti-mildew effect test of mortar is carried out according to the standard GB1741-2007.
[0132] Table 1
[0133] Serial number Contact angle / ° 28-day compressive strength / MPa Mildew resistance Example 1 143.8 18.5 Level 0 Example 2 138.4 17.6 Level 0 Example 3 139.7 18.0 Level 0 Example 4 112.4 14.6 Level 0 Example 5 121.6 15.9 Level 0 Example 6 130.2 18.2 Level 1 Example 7 126.5 18.0 Level 1 Comparative Example 1 100.6 11.9 Level 1
[0134] It can be seen from the results in Table 1 that the mortars prepared in Examples 1-3 have good hydrophobicity, high compressive strength and good mildew resistance.
[0135] Compared with Example 1, Example 4 uses only silane coupling agent to modify hydroxypropyl methylcellulose, which enhances the hydrophobicity to a certain extent, but the hydrophobicity is worse than that of modified hydroxypropyl methylcellulose, and also affects the mechanical properties of the mortar.
[0136] Compared with Example 1, in Example 5, the mass ratio of vinyl tri(2-methoxyethoxy)silane and hydroxypropyl methylcellulose was changed when preparing modified hydroxypropyl methylcellulose, so that the cross-linking effect was reduced and the compressive strength was reduced, which further affected the subsequent modification effect and caused the hydrophobicity to further decrease.
[0137] Compared with Example 1, Example 6 changes the molar ratio of 5-chloro-isothiazoline-3-one and maleic anhydride when preparing the mildew and fungicide, making it difficult for ethyl p-aminobenzenesulfonate in the subsequent step to be completely grafted onto the product obtained in step (1), thereby failing to exert a good mildew and fungicide effect and reducing the hydrophobicity.
[0138] Compared with Example 1, Example 7 uses an equal amount of commercially available 5-chloro-isothiazoline-3-one to replace the mildew and fungicide A, resulting in that 5-chloro-isothiazoline-3-one cannot play a good mildew and fungicide effect and reduces the hydrophobicity.
[0139] Compared with Example 1, Comparative Example 1 uses an equal amount of commercially available hydroxypropyl methylcellulose to replace modified hydroxypropyl methylcellulose A. The lack of hydrophobic groups and the loss of cross-linking structure cause the hydrophobicity and compressive strength of the mortar to deteriorate, and further make the mortar more susceptible to moisture and mildew.
[0140] The above is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present application. Although the present application is disclosed as above in the preferred embodiment, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases. However, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution.
Claims
1. A method for preparing modified hydroxypropyl methylcellulose, It is characterized in that The following steps are included: S1. Place cotton powder in a dispersed system of a mixed solvent, add sodium hydroxide, heat and react for 30-40 minutes under an inert gas atmosphere, cool to 25°C, stir and react for 1-1.5 hours to obtain alkali cellulose; S2. Add propylene oxide and methyl chloride to the alkali cellulose obtained in step S1, heat to 55-65 ° C for 1.5-2h, and heat to 80-90 ° C for 1.5-2h to obtain a material; S3. The material obtained in step S2 is acidified to adjust the pH to neutral, and the solvent is recovered, and then dried and crushed to obtain hydroxypropyl methylcellulose; S4. Vinyl tri(2-methoxyethoxy)silane and deionized water were stirred and mixed, the pH value was adjusted to 2-3, heated to 40-50° C. for hydrolysis for 10-15 h, and then the hydroxypropyl methylcellulose obtained in step S3 was added and stirred to obtain silane-modified hydroxypropyl methylcellulose; S5. Add 6-(allyloxycarbonylamino)-1-hexanol, ammonium persulfate, and solvent to a reaction kettle, heat to 75-85° C., add the silane-modified hydroxypropyl methylcellulose obtained in step S4, stir and react at a constant temperature of 75-85° C. for 3-5 hours, cool to room temperature, adjust the pH value to neutral, wash, and filter to obtain a modified hydroxypropyl methylcellulose intermediate; S6. Add polyvinyl alcohol and deionized water to the reactor, stir and mix, add 25-35wt% hydrogen peroxide solution, stir and react for 30-40min, add the modified hydroxypropyl methylcellulose intermediate obtained in step S5, stir and react for 30-60min, dry, and grind to obtain modified hydroxypropyl methylcellulose.
2. A method for preparing modified hydroxypropyl methylcellulose according to claim 1, It is characterized in that The mass ratio of vinyl tri(2-methoxyethoxy)silane to hydroxypropyl methylcellulose in step S4 is 1:(2-5).
3. A method for preparing modified hydroxypropyl methylcellulose according to claim 1, It is characterized in that The mass ratio of the polyvinyl alcohol, the 25-35wt% hydrogen peroxide solution and the modified hydroxypropyl methylcellulose intermediate in step S6 is 1:(0.01-0.05):(1-2).
4. A modified hydroxypropyl methylcellulose prepared by the preparation method according to any one of claims 1 to 3.
5. Use of the modified hydroxypropyl methylcellulose prepared by the preparation method according to any one of claims 1 to 3 or the modified hydroxypropyl methylcellulose according to claim 4 in mortar, It is characterized in that The mortar comprises the following raw materials in parts by weight: Cement 50-85 parts 6. Use of the modified hydroxypropyl methylcellulose according to claim 5 in mortar, It is characterized in that The preparation method of the mortar comprises the following steps:
1. Mix cement, yellow sand, fly ash and vitrified microspheres evenly and stir to obtain premix 1; 2. adding modified hydroxypropyl methylcellulose, surfactant and polypropylene fiber to the above premix and stirring to obtain premix 2; 3. Add the premix 1 obtained in step 1 to the premix 2 obtained in step 2, then add the mildew-proofing and fungicide, water-reducing agent and defoaming agent to mix, and then put into the dry mixing equipment to obtain mortar.
7. Use of the modified hydroxypropyl methylcellulose according to claim 5 in mortar, It is characterized in that The length of the polypropylene fiber is 5-15 mm.
8. Use of the modified hydroxypropyl methylcellulose according to claim 5 in mortar, It is characterized in that The surfactant is nonylphenol polyoxyethylene ether.
9. Use of the modified hydroxypropyl methylcellulose according to claim 5 in mortar, It is characterized in that The preparation method of the mildew-proofing and fungicide comprises the following steps: (1) adding 5-chloro-isothiazoline-3-one, maleic anhydride and xylene into a reaction kettle, heating to 115-125° C. under an inert gas atmosphere, keeping the temperature for reaction for 7-8 hours, washing and drying to obtain a reactant; (2) Add the reactant obtained in step (1), ethyl para-aminobenzenesulfonate, N,N-dimethylformamide and ethanol to a reaction kettle, then add a carbodiimide condensation agent and an activator, stir, and react for 5-6 hours to obtain a mildew and fungicide.
10. Use of the modified hydroxypropyl methylcellulose according to claim 9 in mortar, It is characterized in that The molar ratio of 5-chloro-isothiazoline-3-one and maleic anhydride in step (1) is 1: (1.1-1.4).
Citation Information
Cited By
Impact-resistant paste slurry with relatively high impact resistance and preparation method of impact-resistant paste slurry
CN121377684A
An impact-resistant paste with high impact resistance and a method for preparing the same