Bio-based water-based acrylate adhesive and preparation method thereof

Aqueous bio-based acrylate adhesives were prepared by means of explosive polymerization and emulsification, which solved the problem of insufficient performance in traditional methods and achieved the preparation of adhesives with high cohesive energy and environmental friendliness.

CN118909200APending Publication Date: 2024-11-08SUZHOU HI TECH ELECTRONICS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410959796.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing bio-based acrylate adhesives are mostly oil-based systems, which make it difficult to meet the requirements of sustainable development, and traditional water-based preparation methods are difficult to obtain high-performance adhesives.

Method used

A water-based acrylate adhesive was prepared by combining a burst polymerization reaction with an emulsification step, which involved heating and mixing bio-based acrylate monomers and an initiator to induce burst polymerization, followed by the addition of an emulsifier and water for emulsification, and then the addition of a nucleation emulsion under heating conditions for further polymerization.

Benefits of technology

A high-cohesive waterborne bio-based acrylate adhesive was prepared, with a narrow molecular weight distribution, reducing the precipitation of small molecules, meeting environmental protection requirements, and improving adhesive performance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a bio-based water-based acrylate adhesive and a preparation method thereof.The preparation method of the bio-based water-based acrylate adhesive comprises the following steps that a mixed system containing a bio-based acrylate monomer and an initiator is heated to be subjected to implosion reaction, and after the reaction is finished, the bio-based water-based acrylate adhesive is obtained; adding a first emulsifier and water into the reaction product for emulsification to obtain an acrylate prepolymer; uniformly mixing and stirring a bio-based acrylate monomer, a second emulsifier and water to obtain a core growth emulsion; and under a heating condition, dropwise adding the core growth emulsion into an acrylate prepolymer, and carrying out a polymerization reaction to obtain the bio-based water-based acrylate adhesive. The bio-based water-based acrylate adhesive and the preparation method thereof have the advantages that the prepared bio-based water-based acrylate adhesive has high cohesive energy, organic solvents are not used in the preparation process, and the bio-based water-based acrylate adhesive is more in line with green and environment-friendly requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of acrylic adhesives, and in particular relates to a bio-based water-based acrylic adhesive and a preparation method thereof. Background Art

[0002] At present, all bio-based acrylates on the market use oily systems, which do not conform to the basic principles of sustainable development. Therefore, in order to prepare bio-based adhesives that conform to the concept of sustainable development, water-based bio-based acrylate adhesives are considered. However, due to the large side groups of bio-based acrylates, the difficulty of free radical polymerization increases, and the cohesive energy is low. It is difficult to obtain glue with good performance by synthesizing bio-based acrylates using traditional water-based acrylate preparation methods.

[0003] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention

[0004] The object of the present invention is to provide a bio-based water-based acrylate adhesive and a preparation method thereof. The prepared bio-based water-based acrylate adhesive has the advantages of high cohesive energy and is more in line with the requirements of green environmental protection.

[0005] In order to achieve the above object, a specific embodiment of the present invention provides a method for preparing a bio-based water-based acrylic adhesive, comprising the following steps:

[0006] The mixed system containing the bio-based acrylate monomer and the initiator is heated to cause an implosion reaction, and after the reaction is completed, a first emulsifier and water are added to the reaction product for emulsification to obtain an acrylate prepolymer;

[0007] The bio-based acrylate monomer, the second emulsifier and water are mixed and stirred to obtain a core growth emulsion;

[0008] Under heating conditions, the core growth emulsion is added dropwise to the acrylate prepolymer to carry out a polymerization reaction to obtain a bio-based water-based acrylate adhesive.

[0009] In one or more embodiments of the present invention, in the mixed system, the mass ratio of the bio-based acrylate monomer to the initiator is (30-35): (0.3-1).

[0010] In one or more embodiments of the present invention, during the process of adding the first emulsifier and water to the reaction product for emulsification, the mass of the first emulsifier is 0.3% to 0.6% of the mass of the bio-based acrylate monomer.

[0011] In one or more embodiments of the present invention, the heating temperature of the mixed system is 70-75° C., and the reaction time of the implosion reaction is 1.5-2.5 h.

[0012] In one or more embodiments of the present invention, the first emulsifier is at least one of sodium hexadecyl sulfonate, ammonium persulfate, and sodium methyl bicarbonate; and / or,

[0013] The second emulsifier is at least one of sodium hexadecyl sulfate, ammonium persulfate, and sodium methyl bicarbonate.

[0014] In one or more embodiments of the present invention, the initiator is at least one of azobisisobutylcyanide and dimethyl azobisisobutyrate.

[0015] In one or more embodiments of the present invention, the bio-based acrylate monomer is at least one of lauryl acrylate, tetrahydrofurfuryl acrylate, tridecyl acrylate, and octyl acrylate.

[0016] In one or more embodiments of the present invention, in the step of preparing the core growth emulsion, the mass ratio of the bio-based acrylate monomer to water is (30-35): (65-70), and the mass of the second emulsifier is 0.3% to 0.6% of the mass of the bio-based acrylate monomer.

[0017] In one or more embodiments of the present invention, the core growth emulsion is added dropwise to the acrylate prepolymer under heating conditions to carry out a polymerization reaction, comprising:

[0018] Under the condition of 75-80° C., the core growth emulsion is added dropwise to the acrylate prepolymer for polymerization reaction. The adding time is 1-1.5 hours. After the adding is completed, the temperature is kept for 2-2.5 hours.

[0019] A specific embodiment of the present invention provides a bio-based water-based acrylate adhesive prepared by the above-mentioned method for preparing the bio-based water-based acrylate adhesive.

[0020] Compared with the prior art, the bio-based water-based acrylic adhesive and the preparation method thereof of the present invention have the following beneficial effects:

[0021] (1) Currently, all bio-based acrylate adhesives on the market use an oily system, which requires the use of a large amount of organic solvents, which is inconsistent with the original intention of using bio-based acrylates to protect the environment. The bio-based acrylate adhesive of the present invention is a water-based system, that is, water is used as a solvent, which complies with national policy standards, compared with oily bio-based acrylates.

[0022] (2) The molecular weight of the bio-based acrylate polymer can be increased through the implosion reaction, and then the subsequent core growth emulsion can be used to continue the polymerization, which can not only further increase the molecular weight of the bio-based acrylate polymer and increase the cohesive energy of the entire adhesive, but also narrow the molecular weight distribution of the bio-based acrylate polymer. The narrowing of the molecular weight distribution will reduce the content of small molecules in the colloid, reduce the precipitation and pollution of small molecules during use, and have better overall performance. DETAILED DESCRIPTION

[0023] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0024] At present, all bio-based acrylates on the market use oily systems, which do not conform to the basic principles of sustainable development. Therefore, in order to prepare bio-based adhesives that conform to the concept of sustainable development, water-based bio-based acrylate adhesives are considered. However, due to the large side groups of bio-based acrylates, the difficulty of free radical polymerization increases, and the cohesive energy is low. It is difficult to obtain glue with good performance by synthesizing bio-based acrylates using traditional water-based acrylate preparation methods.

[0025] The preparation method of the bio-based water-based acrylic adhesive in one example of the present invention comprises the following steps:

[0026] S1, heating a mixed system containing a bio-based acrylate monomer and an initiator to cause an implosion reaction, and after the reaction is completed, adding a first emulsifier and water to the reaction product for emulsification to obtain an acrylate prepolymer;

[0027] S2, mixing and stirring the bio-based acrylate monomer, the second emulsifier and water to obtain a core growth emulsion;

[0028] S3. Under heating conditions, dropwise adding the core growth emulsion into the acrylate prepolymer to carry out polymerization reaction to obtain a bio-based water-based acrylate adhesive.

[0029] It should be noted that the order of steps S1 and S2 can be swapped, that is, step S1 can be performed first and then step S2, or step S2 can be performed first and then step S1, or step S1 and step S2 can be performed simultaneously.

[0030] It should be noted that, since the molecular weight of the common bio-based acrylate monomers is very low, it is difficult to polymerize high molecular weight bio-based acrylate polymers using conventional polymerization methods. Therefore, the present invention adopts bulk polymerization, that is, adding an excessive amount of initiator to initiate implosion without adding a solvent. As the bio-based acrylate monomer is consumed, the implosion phenomenon gradually disappears; the molecular weight distribution of the prepared bio-based acrylate polymer will be very wide, not only there are bio-based acrylate polymers with very low molecular weight, but also there are bio-based acrylate polymers with molecular weight far exceeding the conventional preparation method. In addition, since no organic solvent is added in the above reaction process, the viscosity is high at a certain heating temperature (for example, at about 75°C), and the viscosity will be higher at room temperature. It is necessary to use water and a first emulsifier to emulsify it, reduce the viscosity of the reaction product, and obtain an acrylate prepolymer.

[0031] Then, the core growth emulsion is added dropwise to the above-mentioned acrylate prepolymer, so that the bio-based acrylate polymer in the latex particles in the acrylate prepolymer can continue to grow, further increasing the molecular weight of the bio-based acrylate polymer; wherein, the molecular weight growth rate of the bio-based acrylate polymer with a lower molecular weight in the acrylate prepolymer is greater than the molecular weight growth rate of the bio-based acrylate polymer with a larger molecular weight. Therefore, the core growth emulsion can narrow the molecular weight distribution of the bio-based acrylate polymer in the prepared bio-based water-based acrylate adhesive. The narrowing of the molecular weight distribution can reduce the content of small molecules inside the colloid (adhesive), reduce the precipitation and pollution of small molecules during use, and have better overall performance.

[0032] Preferably, in the mixed system, the mass ratio of the bio-based acrylate monomer to the initiator is (30-35): (0.3-1).

[0033] Preferably, in the process of adding the first emulsifier and water to the reaction product for emulsification, the mass of the first emulsifier is 0.3% to 0.6% of the mass of the bio-based acrylate monomer.

[0034] Preferably, the heating temperature of the mixed system is 70-75° C., and the reaction time of the implosion reaction is 1.5-2.5 h.

[0035] Specifically, bio-based acrylate monomer and initiator are placed in a reaction bottle under a nitrogen environment, and stirred at 70-75°C for reaction. As the implosion reaction occurs and ends, the system temperature will rise to above 110°C and then drop to 70-75°C. The whole process generally ends in about 2 hours, and then the first emulsifier is added, stirring is continued for about 15 minutes, and an appropriate amount of water is added for emulsification, thereby preparing the acrylate prepolymer we need. For example, the mass ratio of bio-based acrylate monomer to water can be (30-35): (65-70).

[0036] Preferably, the first emulsifier is at least one of sodium hexadecyl sulfonate, ammonium persulfate, and sodium methyl bicarbonate; the second emulsifier is at least one of sodium hexadecyl sulfonate, ammonium persulfate, and sodium methyl bicarbonate.

[0037] Preferably, the initiator is at least one of azobisisobutylcyanide and dimethyl azobisisobutyrate.

[0038] Preferably, the bio-based acrylate monomer is at least one of lauryl acrylate, tetrahydrofurfuryl acrylate, tridecyl acrylate, and octyl acrylate.

[0039] Preferably, in the step of preparing the core growth emulsion, the mass ratio of the bio-based acrylate monomer to water is (30-35): (65-70), and the mass of the second emulsifier is 0.3%-0.6% of the mass of the bio-based acrylate monomer (in this step).

[0040] Preferably, the step of preparing the core growth emulsion may be: adding bio-based acrylate monomer, a second emulsifier and water under a nitrogen environment, and preparing the required core growth emulsion by magnetic stirring for 1 hour.

[0041] Preferably, under heating conditions, the core growth emulsion is added dropwise to the acrylate prepolymer to carry out a polymerization reaction, comprising:

[0042] Under the condition of 75-80° C., the core growth emulsion is added dropwise to the acrylate prepolymer for polymerization reaction. The adding time is 1-1.5 hours. After the adding is completed, the temperature is kept for 2-2.5 hours.

[0043] A specific embodiment of the present invention provides a bio-based water-based acrylate adhesive prepared by the above-mentioned method for preparing the bio-based water-based acrylate adhesive.

[0044] The bio-based water-based acrylic adhesive and its preparation process of the present invention will be described in detail below in conjunction with specific examples and comparative examples.

[0045] Example 1

[0046] Preparation of acrylate prepolymer: 35 parts of lauryl acrylate and 0.5 parts of azobisisobutyl cyanide were placed in a reaction bottle under a nitrogen environment, and stirred at 75°C for reaction. As the implosion reaction occurred and ended, the system temperature would rise to above 110°C and then drop to 75°C. The whole process was completed within 2 hours. Sodium dodecyl sulfonate (0.07 parts) with a mass percentage of 0.2% of the bio-based acrylate monomer, ammonium persulfate (0.07 parts) with a mass percentage of 0.2% of the bio-based acrylate monomer, and sodium hydrogen sulfonate (0.07 parts) with a mass percentage of 0.2% of the bio-based acrylate monomer were added. Stirring was continued for 15 minutes, and emulsified with 65 parts of water to prepare the acrylate prepolymer we needed.

[0047] Preparation of core growth emulsion: Under a nitrogen environment, add 35 parts of lauryl acrylate, 0.2% of the mass of bio-based acrylate monomer sodium dodecyl sulfonate (0.07 parts), 0.2% of the mass of bio-based acrylate monomer ammonium persulfate (0.07 parts), 0.2% of the mass of bio-based acrylate monomer sodium hydrogen sulfonate (0.07 parts) and 65 parts of water, and prepare the required core growth emulsion by magnetic stirring for 1 hour.

[0048] Preparation of bio-based water-based acrylic adhesive: 76 parts of acrylic prepolymer were placed in a reaction bottle, and 24 parts of core growth emulsion were added dropwise at 80° C. within 1 hour, and then kept warm for 2 hours to obtain the bio-based water-based acrylic adhesive S1 of the present invention.

[0049] Preparation method of bio-based water-based acrylic adhesive tape: First, mix commercially available polyethylenimine crosslinker SAC-100 and deionized water, and prepare the adhesive mixture according to the ratio of bio-based water-based acrylic adhesive S1: crosslinker SAC-100: solvent deionized water = 100: 0.5: 25. Secondly, coat it on the heavy release film, let it stand in an oven at 120°C for 3 minutes, take it out and cover it with a light release film.

[0050] Example 2

[0051] Preparation of acrylate prepolymer: 33 parts of tridecyl acrylate and 0.7 parts of dimethyl azobisisobutyrate were placed in a reaction bottle under a nitrogen environment, and stirred at 75°C for reaction. As the implosion reaction occurred and ended, the system temperature rose to above 110°C and then dropped to 73°C. The whole process was completed within 2 hours. 0.1% of sodium dodecyl sulfonate, 0.1% of ammonium persulfate, and 0.2% of sodium hydrogen sulfonate were added, and stirring was continued for 15 minutes. Emulsification was performed with 67 parts of water, thereby preparing the acrylate prepolymer we needed.

[0052] Preparation of core growth emulsion: 33 parts of tridecyl acrylate, 0.1% of sodium dodecyl sulfate, 0.1% of ammonium persulfate, 0.2% of sodium hydrogen sulfonate and 67 parts of water were added under nitrogen environment, and the required core growth emulsion was prepared by magnetic stirring for 1 hour.

[0053] Preparation of bio-based water-based acrylic adhesive: 70 parts of acrylic prepolymer were placed in a reaction bottle, and 30 parts of core growth emulsion were added dropwise at 80° C. within 1 hour, and then kept warm for 2 hours to obtain the bio-based water-based acrylic adhesive S2 of the present invention.

[0054] Preparation method of bio-based water-based acrylic adhesive tape: First, mix commercially available polyethylenimine crosslinker SAC-100 and deionized water, and prepare the adhesive mixture according to the ratio of bio-based water-based acrylic adhesive S2: crosslinker SAC-100: solvent deionized water = 100: 0.5: 25. Secondly, coat it on the heavy release film, let it stand in an oven at 120°C for 3 minutes, take it out and cover it with a light release film.

[0055] Example 3

[0056] Preparation of acrylate prepolymer: 30 parts of tetrahydrofurfuryl acrylate and 1 part of dimethyl azobisisobutyrate were placed in a reaction bottle under a nitrogen environment, and stirred at 70°C for reaction. As the implosion reaction occurred and ended, the system temperature rose to above 110°C and then dropped to 70°C. The whole process was completed within 2 hours. 0.15% of sodium dodecyl sulfate, 0.15% of ammonium persulfate, and 0.3% of sodium hydrogen sulfonate were added, and stirring was continued for 15 minutes. Emulsification was performed with 70 parts of water, thereby preparing the acrylate prepolymer we needed.

[0057] Preparation of nuclear growth emulsion: Add 30 parts of tetrahydrofurfuryl acrylate, 0.15% of sodium dodecyl sulfate, 0.15% of ammonium persulfate, 0.3% of sodium hydrogen sulfonate and 70 parts of water under nitrogen environment, and prepare the required nuclear growth emulsion by magnetic stirring for 1 hour.

[0058] Preparation of bio-based water-based acrylate adhesive: 80 parts of acrylate prepolymer are placed in a reaction bottle, and 20 parts of core growth emulsion are added dropwise at 80° C. within 1 hour, and then the mixture is kept warm for 2 hours, thereby obtaining the bio-based water-based acrylate adhesive S3 of the present invention.

[0059] Preparation method of bio-based water-based acrylic adhesive tape: First, mix commercially available polyethylenimine crosslinker SAC-100 and deionized water, and prepare the adhesive mixture according to the ratio of bio-based water-based acrylic adhesive S3: crosslinker SAC-100: solvent deionized water = 100: 0.5: 25. Secondly, coat it on the heavy release film, let it stand in an oven at 120°C for 3 minutes, take it out and cover it with a light release film.

[0060] Comparative Example 1

[0061] Preparation of traditional solvent-based acrylic ester: 35 parts of lauryl acrylate, 0.5 parts of azobisisobutyl cyanide, and 75 parts of ethyl acetate were placed in a reaction bottle under nitrogen and stirred at 65°C. The reaction was carried out for 12 hours, and the viscosity of the glue gradually increased. After the reaction was completed, air was slowly introduced into the glue. Thus, the solvent-based polyacrylate E1 we needed was prepared.

[0062] Preparation method of solvent-based polyacrylate adhesive tape: First, mix commercially available polyethylenimine crosslinker SAC-100 and ethyl acetate, and prepare the adhesive mixture according to the ratio of bio-based water-based acrylic adhesive E1: crosslinker SAC-100: solvent ethyl acetate = 100: 0.5: 25. Secondly, coat it on the heavy release film, let it stand in an oven at 120°C for 3 minutes, take it out and cover it with a light release film.

[0063] Comparative Example 2

[0064] Preparation of traditional solvent-based acrylic acid ester: 33 parts of tridecyl acrylate, 0.7 parts of dimethyl azobisisobutyrate, and 75 parts of ethyl acetate were placed in a reaction bottle under nitrogen and stirred at 65°C. The reaction was carried out for 12 hours, and the viscosity of the glue gradually increased. After the reaction was completed, air was slowly introduced into the glue. Thus, the solvent-based polyacrylate E2 we needed was prepared.

[0065] Preparation method of solvent-based polyacrylate adhesive tape: First, mix commercially available polyethylenimine crosslinker SAC-100 and ethyl acetate, and prepare the adhesive mixture according to the ratio of bio-based water-based acrylic adhesive E2: crosslinker SAC-100: solvent ethyl acetate = 100: 0.5: 25. Secondly, coat it on the heavy release film, let it stand in an oven at 120°C for 3 minutes, take it out and cover it with a light release film.

[0066] Comparative Example 3

[0067] Preparation of traditional solvent-based acrylic acid ester: 30 parts of tetrahydrofurfuryl acrylate, 1 part of dimethyl azobisisobutyrate, and 75 parts of ethyl acetate were placed in a reaction bottle under nitrogen atmosphere and stirred at 65°C. The reaction was carried out for 12 hours, and the viscosity of the adhesive gradually increased. After the reaction was completed, air was slowly introduced into the adhesive. Thus, the solvent-based polyacrylate E3 we needed was prepared.

[0068] Preparation method of solvent-based polyacrylate adhesive tape: First, mix commercially available polyethylenimine crosslinker SAC-100 and ethyl acetate, and prepare the adhesive mixture according to the ratio of bio-based water-based acrylic adhesive E3: crosslinker SAC-100: solvent ethyl acetate = 100: 0.5: 25. Secondly, coat it on the heavy release film, let it stand in an oven at 120°C for 3 minutes, take it out and cover it with a light release film.

[0069] The following performance tests were performed on the above Examples 1 to 3 and Comparative Examples 1 to 3:

[0070] 1) Viscosity of adhesive: refer to GB / T 2794-2013 Determination of viscosity of adhesives-single cylinder rotational viscometer method.

[0071] 2) Dynamic shear force: refer to GB / T 33332-2016 test method for dynamic shear strength of adhesive tape.

[0072] The following table data is obtained:

[0073] Solid content (%) Glue viscosity (cps) Dynamic shear stress (MPa) Example 1 35% 498 0.724 Example 2 33% 564 0.823 Example 3 30% 518 0.702 Comparative Example 1 31% 2512 0.469 Comparative Example 2 30% 2978 0.425 Comparative Example 3 28% 3263 0.401

[0074] From the comparison between Example 1 and Comparative Example 1, Example 2 and Comparative Example 2, and Example 3 and Comparative Example 3 in the above table, it can be seen that compared with the traditional solvent preparation method, the dynamic shear force of the bio-based water-based acrylate adhesive prepared by the preparation method of the present invention is greatly improved by more than 50%. The greater the dynamic shear, the better the cohesion.

[0075] Compared with the prior art, the bio-based water-based acrylic adhesive and the preparation method thereof of the present invention have the following beneficial effects:

[0076] (1) Currently, all bio-based acrylate adhesives on the market use an oily system, which requires the use of a large amount of organic solvents, which is inconsistent with the original intention of using bio-based acrylates to protect the environment. The bio-based acrylate adhesive of the present invention is a water-based system, that is, water is used as a solvent, which complies with national policy standards, compared with oily bio-based acrylates.

[0077] (2) The molecular weight of the bio-based acrylate polymer can be increased through the implosion reaction, and then the subsequent core growth emulsion can be used to continue the polymerization, which can not only further increase the molecular weight of the bio-based acrylate polymer and increase the cohesive energy of the entire adhesive, but also narrow the molecular weight distribution of the bio-based acrylate polymer and improve the overall performance.

[0078] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0079] In addition, it should be understood that although this specification is described in terms of implementation methods, not every implementation method contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other implementation methods that can be understood by those skilled in the art.

Claims

1. A method for preparing a bio-based water-based acrylic adhesive, characterized in that: The following steps are involved: The mixed system containing the bio-based acrylate monomer and the initiator is heated to cause an implosion reaction, and after the reaction is completed, a first emulsifier and water are added to the reaction product for emulsification to obtain an acrylate prepolymer; The bio-based acrylate monomer, the second emulsifier and water are mixed and stirred to obtain a core growth emulsion; Under heating conditions, the core growth emulsion is added dropwise to the acrylate prepolymer to carry out a polymerization reaction to obtain a bio-based water-based acrylate adhesive.

2. The method for preparing the bio-based water-based acrylic adhesive according to claim 1, characterized in that: In the mixed system, the mass ratio of the bio-based acrylate monomer to the initiator is (30-35): (0.3-1).

3. The method for preparing the bio-based water-based acrylic adhesive according to claim 1, characterized in that: In the process of adding the first emulsifier and water to the reaction product for emulsification, the mass of the first emulsifier is 0.3% to 0.6% of the mass of the bio-based acrylate monomer.

4. The method for preparing the bio-based water-based acrylic adhesive according to claim 1, characterized in that: The heating temperature of the mixed system is 70-75° C., and the reaction time of the implosion reaction is 1.5-2.5 hours.

5. The method for preparing the bio-based water-based acrylic adhesive according to claim 1, characterized in that: The first emulsifier is at least one of sodium hexadecyl sulfonate, ammonium persulfate, and sodium methyl bicarbonate; and / or, The second emulsifier is at least one of sodium hexadecyl sulfate, ammonium persulfate, and sodium methyl bicarbonate.

6. The method for preparing the bio-based water-based acrylic adhesive according to claim 1, characterized in that: The initiator is at least one of azobisisobutylcyanide and dimethyl azobisisobutyrate.

7. The method for preparing the bio-based water-based acrylic adhesive according to claim 1, characterized in that: The bio-based acrylate monomer is at least one of lauryl acrylate, tetrahydrofurfuryl acrylate, tridecanol acrylate, and octyl acrylate.

8. The method for preparing the bio-based water-based acrylic adhesive according to claim 1, characterized in that: In the step of preparing the core growth emulsion, the mass ratio of the bio-based acrylate monomer to water is (30-35): (65-70), and the mass of the second emulsifier is 0.3%-0.6% of the mass of the bio-based acrylate monomer.

9. The method for preparing the bio-based water-based acrylic adhesive according to claim 1, characterized in that: Under heating conditions, the core growth emulsion is added dropwise to the acrylate prepolymer to carry out a polymerization reaction, including: Under the condition of 75-80° C., the core growth emulsion is added dropwise to the acrylate prepolymer for polymerization reaction. The adding time is 1-1.5 hours. After the adding is completed, the temperature is kept for 2-2.5 hours.

10. A bio-based water-based acrylic adhesive, characterized in that: The bio-based water-based acrylate adhesive is prepared by the preparation method of the bio-based water-based acrylate adhesive according to any one of claims 1 to 9.