Water-based polyurethane ink binder for ink-jet printing as well as preparation method and application of water-based polyurethane ink binder

The synthesis of aqueous polyurethane ink bonding materials by two-step polymerization method solves the problem of inkjet printing ink ink ink ink, improves the stability and bonding strength of the film layer, and achieves the performance improvement of water-based ink suitable for inkjet printing, avoiding the Environmental pollution of solvent-based inks.

CN118909222APending Publication Date: 2024-11-08JINGCHU UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411112628.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing inks are not suitable for inkjet printing. The film layer prepared by water-based polyurethane is prone to cracking, which limits the application of printing materials. In addition, water-based inks do not meet the standards in printing performance and quality, making it difficult to use in high gloss occasions.

Method used

The aqueous polyurethane ink linking material is synthesized by two-step polymerization using isophorone diisocyanate, polycaprolactone diol and 2,2-dihydroxymethylbutyric acid, and added with hydrophilic chain extender and viscosity regulator. Adjust the reaction conditions to improve the stability and bonding strength of the adhesive film.

Benefits of technology

It has successfully improved the water absorption and bonding strength of the water-based polyurethane ink, enhanced the dispersion performance, is suitable for inkjet printing, and has a moderate viscosity, and is suitable for ink preparation, avoiding the pollution of the environment by solvent-based inks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909222A_ABST
    Figure CN118909222A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of water-based ink for ink-jet printing, and discloses a water-based polyurethane ink binder for ink-jet printing as well as a preparation method and application of the water-based polyurethane ink binder. At present, most of water-based ink for ink jet in the market is poor in performance, and isophorone diisocyanate and polycaprolactone dihydric alcohol are adopted as main synthesis raw materials, and a water-based polyurethane ink vehicle is synthesized through a two-step polymerization method. Along with the increase of the content of the hydrophilic chain extender, the appearance of the waterborne polyurethane is gradually changed from milky white to slightly white and then to be transparent, and the viscosity of the system is increased; along with the rising of the chain extension temperature, the stability of the system is not obviously changed, the water absorption performance of the adhesive film is firstly increased and then reduced, the bonding strength of the adhesive film is gradually increased, and when the temperature for the reaction by adding the hydrophilic chain extender for the second time is 50 DEG C, the performance of the synthesized dispersion is the best.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of water-based ink for inkjet printing, and in particular to a water-based polyurethane ink vehicle for inkjet printing, and a preparation method and application thereof. Background Art

[0002] Inkjet printing is a plateless and pressureless printing method that forms image and text information under the control of a computer. The pressure causes the liquid ink to form ink droplets, and the ink flow is sprayed onto the surface of the substrate. Inkjet printing can be quickly printed on substrates of various shapes and surfaces. The inkjet printing process is simple, eliminating the complicated pre-press processes of traditional printing (phototypesetting, platemaking, copying, and platemaking), shortening the production cycle, reducing costs, and reducing pollution. Inkjet digital printing is a new printing method developed innovatively by the printing industry and an era trend in the development of printing technology.

[0003] Compared with traditional printing inks, inkjet printing inks have higher requirements for ink quality, but the amount of use is not large, domestic production is small and the quality is poor, and most of them rely on imports; the water-based inks currently used in the printing field are mostly water-based plastic gravure inks and water-based tipping paper gravure inks. The application range is not comprehensive enough, and the main application is concentrated in traditional printing methods. In addition, water-based inks still have certain technical limitations, and their printing performance and quality do not meet the standards of solvent-based inkjet printing inks; due to the high surface tension of water, the ink is difficult to wet and the drying rate is slow, making it difficult for water-based inks to have a good wetting and printing effect on most substrates, and there are disadvantages such as poor resistance and easy to cause paper shrinkage. In addition, due to the fact that water-based inks are not resistant to sunlight and water, the glossiness of water-based inks is also lower than that of solvent-based inks, which greatly limits the use of water-based inks in actual production and life, even in occasions with high gloss requirements. However, compared with water-based inks, solvent-based inks contain a large amount of volatile organic compounds, which seriously damage human health and the ecological environment. As people's environmental awareness increases, the practice of sacrificing the natural environment in exchange for economic benefits has gradually been replaced and prohibited. It is very necessary to study new environmentally friendly water-based inks for inkjet, which is of great significance in the printing and packaging industry.

[0004] Waterborne polyurethane (WPU) has the advantages of excellent mechanical properties, easy modification, good compatibility with pigments, safety and pollution-free during application. Therefore, ink with waterborne polyurethane as a binder is one of the most promising printing inks on the market. In the process of preparing waterborne polyurethane, although the experimental process was improved and an oil-soluble initiator was used, the obtained emulsion had certain improvements in performance and yield. However, there are also some problems: when different types of emulsions are made into films, the film layer of the sample has cracking phenomena, and its substrate is subject to certain restrictions; and the requirements for inks in inkjet printing and traditional printing methods are completely different and cannot be universal. Therefore, it is necessary to study waterborne polyurethane ink binders for inkjet printing, and it also has certain reference value for research on inkjet printing thin film products, such as inkjet printing batteries, inkjet printing flexible circuits, etc. Summary of the invention

[0005] The purpose of the present invention is to provide an aqueous polyurethane ink vehicle for inkjet printing and a preparation method and application thereof, so as to solve the problem that traditional inks are not suitable for inkjet printing and the film layer prepared by existing aqueous polyurethane is easy to crack, thereby limiting the printing substrate.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing a water-based polyurethane ink vehicle for inkjet printing, comprising the following steps:

[0008] (1) polycaprolactone diol and isophorone diisocyanate are mixed and a first reaction is carried out at 65-70° C. for 0.3-0.6 h; then dibutyltin dilaurate is added and the temperature is raised to 75-80° C. for a second reaction for 1.6-2.2 h;

[0009] (2) After all -OH groups have reacted, add a hydrophilic chain extender and a viscosity modifier, and continue the third reaction at 75-80°C for 2-3 hours;

[0010] (3) cooling the product obtained in step (2) to 30-70° C., adding a hydrophilic chain extender and a viscosity modifier again, and performing a fourth reaction for 0.8-1.2 h;

[0011] (4) The product obtained in step (3) is adjusted to a temperature of 40 to 45° C., the pH value of the system is adjusted to 7 to 8, and the product is mixed with water for emulsification to obtain a water-based polyurethane ink vehicle.

[0012] Preferably, in the method for preparing a water-based polyurethane ink vehicle for inkjet printing, the polycaprolactone diol in step (1) is PCL-1000; and the auxiliary agent for adjusting the pH value of the system in step (4) is triethanolamine.

[0013] Preferably, in the method for preparing a water-based polyurethane ink vehicle for inkjet printing, the hydrophilic chain extender in step (2) and the hydrophilic chain extender in step (3) are 2,2-dihydroxymethylbutyric acid, and the viscosity modifier in step (2) and the viscosity modifier in step (3) are propylene glycol methyl ether acetate.

[0014] Preferably, in the method for preparing a water-based polyurethane ink vehicle for inkjet printing, the mass ratio of the polycaprolactone diol to the isophorone diisocyanate in step (1) is 1:0.45-0.5; the mass ratio of the polycaprolactone diol to the dibutyltin dilaurate in step (1) is 1:0.004-0.005.

[0015] Preferably, in the method for preparing a water-based polyurethane ink vehicle for inkjet printing, the mass ratio of the polycaprolactone diol in step (1), the hydrophilic chain extender in step (2), and the viscosity regulator in step (2) is 1:0.1-0.24:0.075-0.15; the mass ratio of the polycaprolactone diol in step (1), the hydrophilic chain extender in step (3), and the viscosity regulator in step (3) is 1:0.1-0.24:0.075-0.15.

[0016] Preferably, in the method for preparing a water-based polyurethane ink vehicle for inkjet printing, the mass ratio of the polycaprolactone diol in step (1) to the water in step (4) is 1 to 2:1.

[0017] Preferably, in the method for preparing a water-based polyurethane ink vehicle for inkjet printing, the stirring speeds of the first reaction in step (1), the second reaction in step (1), the third reaction in step (2) and the fourth reaction in step (3) are independently 180 to 200 rpm.

[0018] Preferably, in the method for preparing a water-based polyurethane ink vehicle for inkjet printing, the emulsification temperature in step (4) is 30 to 50°C, the stirring speed of the emulsification in step (4) is 1000 to 1500 rpm, and the emulsification time in step (4) is 20 to 40 min.

[0019] The invention also provides an aqueous polyurethane ink vehicle prepared by the method for preparing the aqueous polyurethane ink vehicle for inkjet printing.

[0020] The invention also provides an application of the aqueous polyurethane ink vehicle in inkjet printing.

[0021] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:

[0022] Most of the water-based inks for inkjet on the market currently have poor performance. The present invention uses isophorone diisocyanate (IPDI), polycaprolactone diol (PCL-1000), and 2,2-dihydroxymethylbutyric acid (DMBA) as the main synthetic raw materials, and synthesizes a water-based polyurethane (WPU) ink vehicle by a two-step polymerization method. With the increase of the content of the hydrophilic chain extender DMBA, the appearance of the water-based polyurethane gradually changes from milky white to slightly white and then to transparent, and the viscosity of the system increases; with the increase of the chain extension temperature, the stability of the system does not change significantly, the water absorption performance of the film increases first and then decreases, and the bonding strength of the film gradually increases. When the temperature of the second addition of the hydrophilic chain extender for reaction is 50°C, the performance of the synthesized dispersion is the best. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required to be used in the description of the embodiments or the prior art are briefly introduced below.

[0024] Figure 1 This is the infrared spectrum of the water-based polyurethane ink vehicle obtained in Example 5;

[0025] Figure 2 The water absorption test results of the films prepared from the water-based polyurethane ink vehicles obtained in Examples 5 to 7;

[0026] Figure 3 These are the test results of the bonding strength of the films prepared from the aqueous polyurethane ink vehicles obtained in Examples 5 to 7. DETAILED DESCRIPTION

[0027] The present invention provides a method for preparing a water-based polyurethane ink vehicle for inkjet printing, comprising the following steps:

[0028] (1) polycaprolactone diol and isophorone diisocyanate are mixed and a first reaction is carried out at 65-70° C. for 0.3-0.6 h; then dibutyltin dilaurate is added and the temperature is raised to 75-80° C. for a second reaction for 1.6-2.2 h;

[0029] (2) After all -OH groups have reacted, add a hydrophilic chain extender and a viscosity modifier, and continue the third reaction at 75-80°C for 2-3 hours;

[0030] (3) cooling the product obtained in step (2) to 30-70° C., adding a hydrophilic chain extender and a viscosity modifier again, and performing a fourth reaction for 0.8-1.2 h;

[0031] (4) The product obtained in step (3) is adjusted to a temperature of 40 to 45° C., the pH value of the system is adjusted to 7 to 8, and the product is mixed with water for emulsification to obtain a water-based polyurethane ink vehicle.

[0032] In the present invention, the polycaprolactone diol in step (1) is preferably PCL-1000.

[0033] In the present invention, the polycaprolactone diol in step (1) is preferably dehydrated before use.

[0034] In the present invention, the dehydration treatment is preferably vacuum drying.

[0035] The present invention does not limit the vacuum drying conditions, and a solution familiar to those skilled in the art can be used. Specifically, in the embodiment of the present invention, the vacuum drying temperature is 110° C., and the vacuum drying time is 2 hours.

[0036] In the present invention, the hydrophilic chain extender in step (2) and the hydrophilic chain extender in step (3) are preferably 2,2-dihydroxymethylbutyric acid.

[0037] In the present invention, the viscosity modifier in step (2) and the viscosity modifier in step (3) are preferably propylene glycol methyl ether acetate.

[0038] In the present invention, the auxiliary agent for adjusting the pH value of the system in step (4) is preferably triethanolamine.

[0039] In the present invention, the mass ratio of the polycaprolactone diol to the isophorone diisocyanate in step (1) is preferably 1:0.45-0.5, more preferably 1:0.46-0.48, and more preferably 1:0.476.

[0040] In the present invention, the mass ratio of the polycaprolactone diol to the dibutyltin dilaurate in step (1) is preferably 1:0.004-0.005, more preferably 1:0.0043-0.0048, and more preferably 1:0.0045.

[0041] In the present invention, the temperature of the first reaction in step (1) is preferably 67-70°C, more preferably 69-70°C, and more preferably 70°C; the time of the first reaction in step (1) is preferably 0.4-0.56h, more preferably 0.48-0.54h, and more preferably 0.5h.

[0042] In the present invention, the temperature of the second reaction in step (1) is preferably 75-79°C, more preferably 75-77°C, and more preferably 75°C; the time of the second reaction in step (1) is preferably 1.8-2.2h, more preferably 1.9-2.1h, and more preferably 2h.

[0043] In the present invention, the mass ratio of the polycaprolactone diol in step (1), the hydrophilic chain extender in step (2), and the viscosity modifier in step (2) is preferably 1:0.1-0.24:0.075-0.15, more preferably 1:0.175-0.24:0.12-0.15, and more preferably 1:0.175:0.15.

[0044] In the present invention, the temperature of the third reaction in step (2) is preferably 75-79°C, more preferably 75-77°C, and more preferably 75°C; the time of the third reaction in step (2) is preferably 2.2-2.8h, more preferably 2.4-2.6h, and more preferably 2.5h.

[0045] In the present invention, the mass ratio of the polycaprolactone diol in step (1), the hydrophilic chain extender in step (3), and the viscosity modifier in step (3) is preferably 1:0.1-0.24:0.075-0.15, more preferably 1:0.175-0.24:0.12-0.15, and more preferably 1:0.175:0.15.

[0046] In the present invention, the temperature of the fourth reaction in step (3) is preferably 40-60°C, more preferably 45-55°C, and more preferably 50°C; the time of the fourth reaction in step (3) is preferably 0.85-1.1h, more preferably 0.95-1.05h, and more preferably 1h.

[0047] In the present invention, the end point of adjusting the temperature of the product obtained in step (3) in step (4) is preferably 42 to 45°C, more preferably 44 to 45°C, and even more preferably 45°C.

[0048] In the present invention, the end point of the pH value of the adjustment system in step (4) is preferably 7.2 to 7.8, more preferably 7.4 to 7.6, and even more preferably 7.5.

[0049] In the present invention, the mass ratio of the polycaprolactone diol in step (1) to the water in step (4) is preferably 1 to 2:1, more preferably 1.5 to 2:1, and even more preferably 2:1.

[0050] In the present invention, the emulsification temperature in step (4) is preferably 30-50°C, more preferably 40-45°C, and more preferably 40°C; the stirring speed in step (4) is preferably 1000-1500rpm, more preferably 1100-1300rpm, and more preferably 1200rpm; the emulsification time in step (4) is preferably 20-40min, more preferably 25-35min, and more preferably 30min.

[0051] In the present invention, the stirring speed of the first reaction in step (1), the second reaction in step (1), the third reaction in step (2) and the fourth reaction in step (3) is independently preferably 180 to 200 rpm, more preferably 190 to 200 rpm, and more preferably 200 rpm.

[0052] The invention also provides an aqueous polyurethane ink vehicle prepared by the method for preparing the aqueous polyurethane ink vehicle for inkjet printing.

[0053] The present invention also provides an application of the aqueous polyurethane ink vehicle in inkjet printing. The present invention does not limit the application method, and any method known to those skilled in the art can be used.

[0054] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0055] Example 1

[0056] This embodiment provides a method for preparing a water-based polyurethane ink vehicle for inkjet printing, comprising the following steps:

[0057] (1) PCL-1000 was vacuum dried at 110°C for 2 h for dehydration;

[0058] 20g of dehydrated PCL-1000 was mixed with 9.25g of isophorone diisocyanate, and reacted at 200rpm and 70℃ for 0.5h; then 0.09g of dibutyltin dilaurate was added, the temperature was raised to 75℃, and the reaction was carried out at 200rpm for 2h;

[0059] (2) After all -OH groups in the reaction system have participated in the reaction, 2 g of a hydrophilic chain extender, 2,2-dihydroxymethylbutyric acid, and 1.5 g of a viscosity regulator, propylene glycol methyl ether acetate, are added to control the viscosity of the reaction system, and the reaction is continued at 200 rpm and 75 °C for 2.5 h;

[0060] (3) cooling the product obtained in step (2) to 50° C., diluting 2 g of the hydrophilic chain extender 2,2-dimethylolbutyric acid with 1.5 g of the viscosity modifier propylene glycol methyl ether acetate, and adding the mixture to the product of step (2), and continuing the reaction at 200 rpm for 1 h;

[0061] (4) The product obtained in step (3) was adjusted to a temperature of 45° C., the pH value of the system was adjusted to 8 using triethanolamine, mixed with 10 g of deionized water, and emulsified at 40° C. and 1200 rpm for 30 min to obtain a water-based polyurethane ink vehicle, which was recorded as Formula A.

[0062] Example 2

[0063] This embodiment provides a method for preparing a water-based polyurethane ink vehicle for inkjet printing, which differs from Embodiment 1 in that the end point of adjusting the pH value of the system in step (4) is changed to 7.5, and other parameter conditions are the same as those in Embodiment 1, recorded as Formula B.

[0064] Example 3

[0065] This embodiment provides a method for preparing a water-based polyurethane ink vehicle for inkjet printing, which differs from Embodiment 1 in that the end point of adjusting the pH value of the system in step (4) is changed to 7.5, and other parameter conditions are the same as those in Embodiment 1, recorded as Formula C.

[0066] Example 4

[0067] The present embodiment provides a method for preparing a water-based polyurethane ink vehicle for inkjet printing, which differs from the embodiment 1 in that: the mass of the hydrophilic chain extender 2,2-dihydroxymethylbutyric acid in step (2) and step (3) is changed to 3.5 g, and the mass of the viscosity modifier propylene glycol methyl ether acetate in step (2) and step (3) is changed to 3 g; the end point of adjusting the pH value of the system in step (4) is changed to 7.5, and the other parameter conditions are the same as those in embodiment 1, recorded as formula D.

[0068] Example 5

[0069] The present embodiment provides a method for preparing a water-based polyurethane ink vehicle for inkjet printing, which differs from the embodiment 1 in that: the mass of the hydrophilic chain extender 2,2-dihydroxymethylbutyric acid in step (2) and step (3) is changed to 4.8 g, and the mass of the viscosity modifier propylene glycol methyl ether acetate in step (2) and step (3) is changed to 3 g; the end point of the pH value of the system in step (4) is changed to 7, and the other parameter conditions are the same as those in embodiment 1, recorded as formula E1.

[0070] Example 6

[0071] This embodiment provides a method for preparing a water-based polyurethane ink vehicle for inkjet printing, which differs from Embodiment 5 in that in step (3), the end point of cooling the product obtained in step (2) is modified to 30°C, and other parameter conditions are the same as those in Embodiment 5, recorded as Formula E2.

[0072] Example 7

[0073] This embodiment provides a method for preparing a water-based polyurethane ink vehicle for inkjet printing, which differs from Embodiment 5 in that in step (3), the end point of cooling the product obtained in step (2) is modified to 70°C, and other parameter conditions are the same as those in Embodiment 5, recorded as Formula E3.

[0074] The aqueous polyurethane ink vehicle obtained in Example 5 was characterized using an IS50 FT-IR infrared spectrometer. The results are as follows: Figure 1 As shown. Figure 1 It can be seen that 3444.13cm -1 The stretching vibration peak of NH is at 1644.76cm, indicating that the -NCO group and -OH group reacted; -1 The peak at 1731-2955cm is the stretching vibration peak of C=O in urea, indicating that when the prepolymer is emulsified in water, -NCO and -NH groups react to extend the chain and produce waterborne polyurethane-urea; 1731-2955cm -1 There is no obvious characteristic peak between -NCO and -NCO, indicating that -NCO has been basically completely reacted. In summary, the scheme of the present invention successfully synthesizes the water-based polyurethane ink vehicle of the expected structure.

[0075] The water-based polyurethane ink vehicle obtained in Examples 3 to 5 was left to stand for 6 months for storage testing to study the effect of the amount of hydrophilic chain extender on the storage stability of the water-based polyurethane ink vehicle. The results are shown in Table 1.

[0076] Table 1. Storage stability results of aqueous polyurethane ink vehicles obtained in Examples 3 to 5

[0077]

[0078] As can be seen from Table 1, when the DMBA content increases, the appearance of the waterborne polyurethane changes from slightly white to transparent. In the prior art, when the size of the latex particles is below 1nm, the dispersion is transparent; when the size of the latex particles is below 100nm, the dispersion is a blue liquid; when the size of the latex particles is above 100nm, the dispersion is milky white. Therefore, the more DMBA content, the smaller the size of the particles in the dispersion system. This is because when the DMBA content increases, the ionizable groups in the system increase, which are connected to the corresponding polyurethane backbone chains, enhancing the hydrophilicity, making it easier to produce shearing during dispersion, and forming small-sized waterborne polyurethane particles. It can also be seen in Table 1 that the storage stability of the waterborne polyurethane dispersion is enhanced as the DMBA content increases. When the DMBA content increases, the hydrophilicity in the system is enhanced, the degree of self-emulsification is enhanced, the emulsion particle size is reduced, it is not easy to produce stratification, and a stable dispersion system can be formed; at the same time, it is not easy to cross-link and entangle the polyurethane macromolecular chain during the dispersion process, which enhances the dispersion success rate.

[0079] The viscosity of the aqueous polyurethane ink vehicle obtained in Examples 1 to 5 was tested as follows: the test was conducted at 25° C. and a rotor speed of 100 rpm. The results are shown in Table 2.

[0080] Table 2. Viscosity results of aqueous polyurethane ink vehicles obtained in Examples 1 to 5

[0081]

[0082] As can be seen from Figure 2, the viscosity of the prepared water-based polyurethane ink vehicle is between 4 and 9 mPa.s, which is suitable for inkjet printing. When the content of DMBA is low, the content of hydrophilic groups in the water-based polyurethane is reduced, the effect of the self-emulsification process is poor, it is difficult to form a stable emulsion, and the synthesized dispersion is easy to stratify; when the content of DMBA is too high, the viscosity of the prepolymer during synthesis is very high, and the polyurethane macromolecular chains are easy to entangle during the dispersion stage. The viscosity of water-based polyurethane is mainly related to the content of DMBA, which is due to its double electric layer and particle structure.

[0083] The water-based polyurethane ink vehicle obtained in Examples 1 to 5 was subjected to a drying test as follows: at 25°C, the water-based polyurethane ink vehicle was applied to the surfaces of ordinary printing paper, 150g coated paper, PE plastic, and glass sheets, respectively, and then a filter paper was used to stick to the surface at regular intervals to determine the drying time. The results are shown in Table 3.

[0084] Table 3. Drying test results of the aqueous polyurethane ink vehicle obtained in Examples 1 to 5

[0085]

[0086] As can be seen from Table 3, the drying performance of waterborne polyurethane varies greatly on different substrate surfaces. This is because the main drying method of waterborne polyurethane is penetration drying. On the surface of ordinary printing paper and coated paper, the penetration effect of waterborne polyurethane is obvious, and water can easily penetrate into the substrate components, and the drying rate is good. In addition, the water content during dispersion and emulsification has a great influence on the drying performance of waterborne polyurethane. On various substrates, the spreadability of waterborne polyurethane is good.

[0087] The water-based polyurethane ink vehicle obtained in Examples 5 to 7 was left to stand for 6 months for storage testing to study the effect of the cooling end point (i.e., chain extension temperature) in step (3) on the storage stability of the water-based polyurethane ink vehicle. The results are shown in Table 4.

[0088] Table 4. Storage stability results of aqueous polyurethane ink vehicles obtained in Examples 5 to 7

[0089]

[0090] It can be seen from Table 4 that, when other conditions remain unchanged, different chain extension temperatures have little effect on the storage stability of waterborne polyurethane.

[0091] Test Example 1

[0092] Place a clean printing material template on a horizontal operating table, weigh appropriate amounts of the aqueous polyurethane ink linking materials of Examples 1 to 7 and drop them on the template to make the film thickness about 1 to 2 mm, and make the emulsion flow evenly on the template without bubbles; after drying at room temperature for 24 hours, put it in an oven and dry it at 80°C. When the film is transparent in appearance, gently remove the film and put it in a dryer for use.

[0093] The film prepared by the water-based polyurethane ink vehicle obtained in Examples 5 to 7 was tested for water absorption rate. The operation was as follows: weigh the film m1 and place it in a beaker, add distilled water, take it out every 2 hours, quickly wipe it dry and weigh it to obtain m2, measure it 6 times in a row, and calculate the water absorption rate according to Formula 1:

[0094] Water absorption rate = (m2-m1) / m1×100% Formula 1

[0095] The water absorption test results of the films prepared from the aqueous polyurethane ink vehicle obtained in Examples 5 to 7 are as follows: Figure 2 As shown. Figure 2 It can be seen that when the chain extension temperature of step (3) is low, the water absorption rate of the film is low. This is because when the chain extension temperature is low, the chain extension reaction rate of the small molecule is slow and the chain extension reaction is not sufficient; when the chain extension temperature is high, the chain extension reaction of the small molecule is violent, which will enhance the entanglement of the chain ends and increase the interaction force between molecules. It is difficult for water molecules to diffuse into the interior of the waterborne polyurethane molecules, which reduces the water absorption rate of the film.

[0096] The adhesive film prepared from the aqueous polyurethane ink vehicle obtained in Examples 5 to 7 was tested for its bonding strength. The test was conducted at 25°C with an effective geometric size of 30×4×1 mm and a tensile speed of 300 mm / min. The results are shown in Table 1. Figure 3 As shown. Figure 3 It can be seen that as the chain extension temperature in step (3) increases, the bonding strength of the film also gradually increases. This is because as the chain extension temperature increases, the activity of the macromolecules increases, making the reaction more complete, and the number of HN-COO-bonds and hydrogen bonds generated by the reaction of PCL and IPDI increases. At the same time, the increase in chain extension temperature increases the content of waterborne polyurethane molecules. The interaction between molecules is also an important factor in increasing the bonding strength of the film.

[0097] The films prepared from the aqueous polyurethane ink vehicle obtained in Examples 1 to 5 were placed in a heater respectively, heated at 30°C, 60°C, 80°C, 100°C, 120°C, 160°C, and 180°C, and the state and color changes were observed. Through experiments, it was found that the morphology and color of the five films did not change significantly under the environments of 30°C, 60°C, 80°C, 100°C, 120°C, 160°C, and 180°C, and the thermal stability degradation temperature of the film of the structure type obtained by the present invention was up to 400°C, wherein the degradation temperature of the hard segment was 220-330°C, and the degradation temperature of the soft segment was 330-400°C.

[0098] Test Example 2

[0099] Take 20 mL of the aqueous polyurethane ink vehicle of Examples 1 to 5, 5 g of edible pigment lemon yellow (manufacturer: Hangzhou Zhongyan Technology Co., Ltd.), and 10 mL of distilled water, and prepare inks respectively.

[0100] The inks prepared using the aqueous polyurethane ink vehicle of Examples 1 to 5 were applied on glass sheets. After film formation, they were covered with filter papers soaked in 1wt% HCl solution, 1wt% NaOH solution, 95wt% ethanol solution and water, respectively, and allowed to stand for 24 hours. The covered samples were compared with the uncovered samples, and the filter papers before covering were compared with the filter papers after covering. According to the provisions on the chemical resistance level of ink in Table 5, the levels of acid, alkali, water and solution resistance of the tested samples were judged. The results are shown in Table 6.

[0101] Table 5. Grades of ink chemical resistance

[0102]

[0103] Table 6. Chemical resistance test results of inks prepared from water-based polyurethane ink vehicles obtained in Examples 1 to 5

[0104]

[0105] It can be seen from Table 6 that the ink prepared by the aqueous polyurethane ink vehicle of the present invention has good acid resistance, alkali resistance and water resistance, and shows a slight color change in a 95wt% ethanol solution; the aqueous polyurethane ink vehicle is slightly soluble in water and has a certain water absorption, which is attributed to the local polarity and the number of ionic groups on the surface of the aqueous polyurethane.

[0106] In summary, a series of water-based polyurethane ink vehicles were synthesized by a two-step polymerization method, and the effects of different hydrophilic chain extender contents and different chain extension temperatures on the performance of water-based polyurethane and film were studied. The study found that with the increase of the hydrophilic chain extender content, the appearance of the water-based polyurethane gradually changed from milky white to slightly white and then to transparent, and the viscosity of the system increased. The chain extension temperature was selected at 30°C, 50°C, and 70°C. With the increase of the chain extension temperature, the stability of the system did not change significantly, the water absorption performance of the film increased first and then decreased, and the bonding strength of the film gradually increased. The drying method of the prepared water-based polyurethane is penetration drying, and the film has strong heat resistance; it is slightly soluble in water, and the acid and alkali resistance needs to be improved. The viscosity of the water-based polyurethane ink vehicle synthesized by the present invention is between 4 and 9 mPa.s, and the heat resistance is good. It can be directly used in the preparation of ink without removing the organic solvent.

[0107] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a water-based polyurethane ink vehicle for inkjet printing, characterized in that: The following steps are involved: (1) polycaprolactone diol and isophorone diisocyanate are mixed and a first reaction is carried out at 65-70° C. for 0.3-0.6 h; then dibutyltin dilaurate is added and the temperature is raised to 75-80° C. for a second reaction for 1.6-2.2 h; (2) After all -OH groups have reacted, add a hydrophilic chain extender and a viscosity modifier, and continue the third reaction at 75-80°C for 2-3 hours; (3) cooling the product obtained in step (2) to 30-70° C., adding a hydrophilic chain extender and a viscosity modifier again, and performing a fourth reaction for 0.8-1.2 h; (4) The product obtained in step (3) is adjusted to a temperature of 40 to 45° C., the pH value of the system is adjusted to 7 to 8, and the product is mixed with water for emulsification to obtain a water-based polyurethane ink vehicle.

2. The method for preparing a water-based polyurethane ink vehicle for inkjet printing according to claim 1, characterized in that: The polycaprolactone diol in step (1) is PCL-1000; and the auxiliary agent for adjusting the pH value of the system in step (4) is triethanolamine.

3. The method for preparing a water-based polyurethane ink vehicle for inkjet printing according to claim 1, characterized in that: The hydrophilic chain extender in step (2) and the hydrophilic chain extender in step (3) are 2,2-dihydroxymethylbutyric acid, and the viscosity modifier in step (2) and the viscosity modifier in step (3) are propylene glycol methyl ether acetate.

4. The method for preparing a water-based polyurethane ink vehicle for inkjet printing according to claim 1 or 2, characterized in that: The mass ratio of the polycaprolactone diol to the isophorone diisocyanate in step (1) is 1:0.45-0.5; the mass ratio of the polycaprolactone diol to the dibutyltin dilaurate in step (1) is 1:0.004-0.

005.

5. The method for preparing a water-based polyurethane ink vehicle for inkjet printing according to claim 1 or 3, characterized in that: The mass ratio of the polycaprolactone diol in step (1), the hydrophilic chain extender in step (2), and the viscosity modifier in step (2) is 1:0.1-0.24:0.075-0.15; the mass ratio of the polycaprolactone diol in step (1), the hydrophilic chain extender in step (3), and the viscosity modifier in step (3) is 1:0.1-0.24:0.075-0.

15.

6. The method for preparing a water-based polyurethane ink vehicle for inkjet printing according to claim 1 or 2, characterized in that: The mass ratio of the polycaprolactone diol in step (1) to the water in step (4) is 1 to 2:

1.

7. The method for preparing a water-based polyurethane ink vehicle for inkjet printing according to any one of claims 1 to 3, characterized in that: The stirring speeds of the first reaction in step (1), the second reaction in step (1), the third reaction in step (2) and the fourth reaction in step (3) are independently 180 to 200 rpm.

8. The method for preparing a water-based polyurethane ink vehicle for inkjet printing according to claim 6, characterized in that: The emulsification temperature of step (4) is 30-50° C., the stirring speed of the emulsification of step (4) is 1000-1500 rpm, and the emulsification time of step (4) is 20-40 min.

9. Aqueous polyurethane ink vehicle prepared by the method for preparing an aqueous polyurethane ink vehicle for inkjet printing as claimed in any one of claims 1 to 8.

10. Use of the aqueous polyurethane ink vehicle according to claim 9 in inkjet printing.