Safe and non-toxic medical polymer catalyst, preparation thereof and application of safe and non-toxic medical polymer catalyst in ring-opening polymerization reaction
By preparing an amino acid Schiff base zinc complex catalyst, the problems of insufficient catalytic activity and metal residue in the synthesis of biodegradable materials by zinc-based metal catalysts were solved, and the synthesis of polypropylene glycol copolymer with high catalytic activity and good biocompatibility was achieved.
Patent Information
- Application Number
- CN202410947223.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
In the existing technology, zinc-based metal catalysts do not exhibit excellent catalytic activity in the synthesis of biodegradable materials, and have high metal residues, making it difficult to meet the requirements of safety, non-toxicity, and biocompatibility in the medical field.
Using an amino acid Schiff base zinc complex as a catalyst, an amino acid Schiff base zinc complex is prepared by combining with zinc acetate via a nucleophilic addition reaction. This complex is then used for the ring-opening polymerization of lactide and glycolide, avoiding the use of solvents and achieving highly efficient catalytic synthesis of poly(lactic-co-lactic-co-glycolic acid) copolymers.
It achieves highly efficient ring-opening polymerization reaction with high catalytic activity, high product molecular weight, good thermal stability, easy removal of catalyst residue, and no environmental pollution, meeting the requirements of green environmental protection.
Smart Images

Figure CN118909235A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymers, and in particular to a safe and non-toxic medical polymer catalyst, and its preparation and application in a ring-opening polymerization reaction. Background Art
[0002] Cyclic ester monomers such as caprolactone, glycolide, lactide and carbonate can be used to obtain a class of polymer materials with excellent biocompatibility, biodegradability and absorption through ring-opening polymerization. Among various biodegradable polymers synthesized from renewable resources, polylactic acid and its copolymers are undoubtedly very promising polymers with excellent biodegradability and compatibility. As a completely green and degradable new packaging material, it has been widely used in medical implants, absorbable surgical sutures, drug controlled release systems, fracture internal fixation, etc. It is a safe and efficient polymer medical material.
[0003] Lactide-co-glycolide (PLGA) is one of the most studied degradable polymers. An important characteristic of PLGA is that due to the different properties of poly(glycolide) and poly(lactic acid), the PLGA can have the expected degradation properties by changing the copolymer composition. In addition, there are currently two ways to synthesize poly(glycolide). One is the direct polycondensation method using glycolic acid and lactic acid as raw materials. The copolymer obtained by this method has a low molecular weight and its application is greatly limited. The other is to first make glycolic acid and lactic acid into lactide, and then ring-opening copolymerize to obtain a high molecular weight copolymer. This method mainly has two ways: solution copolymerization and bulk copolymerization. Since solution copolymerization uses a large amount of organic solvents, the most commonly used solvents are benzene, toluene, xylene, etc., which not only requires subsequent complex treatment to remove the solvent, but also does not meet environmental protection requirements, the cost is also high, and it is not suitable for the preparation of poly(glycolide) with a high glycolide content. The bulk copolymerization method avoids the above problems of the solution copolymerization method and is an effective preparation method currently widely used. For example, a Chinese patent (application number 200410018703.3, publication number CN1560109) uses hexabutylguanidine acetate and tetramethyl dibutylguanidine acetate as catalysts to carry out the ring-opening polymerization of cyclic ester monomers. The product obtained in this patent has a low molecular weight, which provides reference and guidance for the development of new non-toxic medical polymer catalysts.
[0004] At present, the commercial production of polylactic acid and polylactic-glycolic acid adopts the ring-opening polymerization method catalyzed by stannous octoate or the polycondensation method catalyzed by stannous chloride. However, the tin compound is not easy to remove from the polymer and has been proven to have certain cytotoxicity. Therefore, it is urgent to find a green catalyst that can be removed from the polymer and is safe and non-toxic to prepare biomedical polymer materials polylactic acid and its copolymers.
[0005] At present, a large number of metal complex catalysts have been reported for the ring-opening polymerization of cyclic ester monomers, including classic main group metals such as magnesium, calcium, aluminum, etc., and transition metals such as copper, cobalt, nickel, zinc, etc. Since transition metals have strong coordination ability and many metals have the ability to change valence, they are widely used in the field of catalysis, but they are also mainly reflected in the fields of asymmetric catalytic cyclopropanation reaction and olefin catalytic oxidation. In the study of biodegradable material synthesis, aluminum-based metal catalysts were used in the early stage for the ring-opening polymerization of cyclic ester monomers, which had good control of molecular weight and stereoselectivity and were widely studied manually. However, since the increase of aluminum concentration is often accompanied by Alzheimer's disease or neurodegenerative diseases, it is affected in biomedical applications and has become less and less popular. Metal catalysts such as magnesium and calcium have also been studied in depth. Although they have good reaction efficiency and good biocompatibility, the high metal residue in the polymer is not easy to remove, which is a major defect. Furthermore, zinc metal is a green catalyst with good biocompatibility, and zinc is an essential metal for the human body, so zinc-based metal catalysts have received more and more attention and research in recent years. The current zinc-based metal complexes are not good enough in catalytic activity, which makes it difficult to regulate their catalytic activity. Therefore, more in-depth research is needed to improve their application value. Biodegradable materials have strict requirements on metal residues and biocompatibility in the medical field. The ideal catalyst residue should be non-toxic or bioabsorbable. The study of safe and non-toxic zinc-based metal catalysts is of great significance for the ring-opening polymerization of cyclic esters. Summary of the invention
[0006] The purpose of the present invention is to provide a safe, non-toxic, and highly efficient ring-opening polymerization catalyst for synthesizing biodegradable medical polyester materials. The method has the characteristics of high reaction conversion rate, good thermal stability, high product molecular weight, and low high-temperature melting degradation. The specific scheme is as follows:
[0007] Firstly, the present invention provides a safe and non-toxic medical polymer catalyst, wherein the catalyst is an amino acid Schiff base zinc complex, and the amino acid comprises one or more of lysine, histidine and arginine.
[0008] Preferably, the amino acid Schiff base zinc complex has the following structures:
[0009]
[0010] Among them, formula (1) is a lysine Schiff base zinc complex, formula (2) is a histidine Schiff base zinc complex, and formula (3) is an arginine Schiff base zinc complex.
[0011] Second, the present invention provides a method for preparing the above-mentioned safe and non-toxic medical polymer catalyst, comprising the following steps:
[0012] (1) adding an amino acid and an inorganic base into a solvent, mixing and stirring, and then adding 3,5-di-tert-butyl salicylaldehyde to carry out a nucleophilic addition reaction to obtain an amino acid Schiff base complex containing an imine group;
[0013] (2) Adding zinc acetate to the product obtained in step (1) to continue the reaction, cooling after the reaction is completed, recrystallizing under low temperature conditions, separating the product, and obtaining a solid powder, which is an amino acid Schiff base zinc complex.
[0014] Preferably, the molar ratio of the amino acid to the inorganic base in step (1) is 1:(1.0-1.4).
[0015] Preferably, the molar ratio of the amino acid to 3,5-di-tert-butyl salicylaldehyde in step (1) is 1:(1.0-1.5).
[0016] Preferably, the molar ratio of the zinc acetate in step (2) to the amino acid bound in the product of step (1) is (1.0-2.0):1.
[0017] Preferably, the solvent in step (1) is methanol.
[0018] Preferably, the ratio of the amount of the amino acid substance in step (1) to the volume of the solvent is (0.01-0.015) mol:50 mL.
[0019] Preferably, the inorganic base in step (1) is sodium hydroxide or potassium hydroxide.
[0020] Preferably, in step (1), the stirring temperature is 20-30° C., the stirring time is 10-30 min, the nucleophilic addition reaction temperature is 55-60° C., and the reaction time is 2-4 h.
[0021] Preferably, the reaction temperature in step (2) is 55-60° C., and the reaction time is 3-5 h.
[0022] Preferably, the recrystallization under low temperature conditions in step (2) is performed at a temperature of 0 to 4° C. for 18 to 24 hours.
[0023] Preferably, the product separation in step (2) includes suction filtration, and the obtained solid is washed 3 to 5 times with anhydrous methanol and then dried.
[0024] Preferably, the amino acids include one or more of lysine, histidine and arginine, specifically:
[0025] In one embodiment of the present invention: a method for preparing a lysine Schiff base zinc complex, the steps of which are: adding lysine and an inorganic base to a methanol solvent, mixing and stirring to dissolve, and then adding 3,5-di-tert-butyl salicylaldehyde to carry out a nucleophilic addition reaction at a specific temperature and time to obtain a lysine Schiff base complex containing an imino group. Subsequently, zinc acetate is added to continue the reaction, and after the reaction is completed, it is placed in a refrigerator, recrystallized under low temperature conditions and allowed to stand for 24 hours, then filtered, washed three times with anhydrous methanol, and dried to obtain a yellow solid powder, which is the lysine Schiff base zinc complex.
[0026] In one embodiment of the present invention: a method for preparing a histidine Schiff base zinc complex, the steps of which are to add histidine and an inorganic base to a methanol solvent, stir and dissolve, and then add 3,5-di-tert-butyl salicylaldehyde to carry out a nucleophilic addition reaction at a specific temperature and time to obtain a histidine Schiff base complex containing an imine group. Subsequently, zinc acetate is added to continue the reaction, and after the reaction is completed, the mixture is placed in a refrigerator, recrystallized under low temperature conditions and allowed to stand for 24 hours, and then filtered, washed three times with anhydrous methanol, and dried to obtain a light yellow solid powder, which is the histidine Schiff base zinc complex.
[0027] In one embodiment of the present invention: a method for preparing an arginine Schiff base zinc complex, the steps of which are to add arginine and an inorganic base to a methanol solvent, mix and stir to dissolve, and then add 3,5-di-tert-butyl salicylaldehyde to carry out a nucleophilic addition reaction at a specific temperature and time to obtain an arginine Schiff base complex containing an imino group. Subsequently, zinc acetate is added to continue the reaction, and after the reaction is completed, the mixture is placed in a refrigerator, recrystallized under low temperature conditions and allowed to stand for 24 hours, then filtered, washed three times with anhydrous methanol, and dried to obtain a brown-red solid powder, which is the arginine Schiff base zinc complex.
[0028] Thirdly, the present invention provides the use of the safe and non-toxic medical polymer catalyst as a catalyst in a ring-opening polymerization reaction.
[0029] Preferably, the ring-opening polymerization reaction in the application comprises a condensation reaction of lactide and glycolide to synthesize a poly(lactide-glycolide) copolymer.
[0030] Preferably, the application comprises: mixing lactide, glycolide and the safe and non-toxic medical polymer catalyst, stirring and heating under reduced pressure to carry out ring-opening polymerization, thereby obtaining poly(lactide-glycolide) copolymer. The method is to carry out ring-opening polymerization by direct melt method to obtain poly(lactide-glycolide) copolymer without adding initiator.
[0031] Preferably, the molar ratio of the catalyst to lactide is 1:(50-5000); the ring-opening polymerization reaction temperature is 100-190°C, preferably 170-175°C; the ring-opening polymerization reaction time is 1-24h, preferably 8h.
[0032] Beneficial effects of the present invention:
[0033] The present invention provides a solvent-free melt copolymerization method for synthesizing a poly(lactide-co-glycolide) copolymer with high biocompatibility, and the catalyst residue in the copolymer is easy to remove. The process provided by the present invention is simple and applicable, does not generate environmental pollutants, and is economical, green and environmentally friendly.
[0034] The invention provides a preparation method of an amino acid Schiff base zinc complex and application of the complex as a catalyst in polymer synthesis. The amino acid Schiff base zinc catalyst provided by the invention has high catalytic activity for the ring-opening polymerization of cyclic ester monomers and good catalytic performance in a wide temperature range. The catalyst provided by the invention can exert a catalytic effect at a relatively low concentration and efficiently catalyze the ring-opening polymerization reaction of lactide and glycolide to synthesize a poly(lactide-glycolide) copolymer. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 is the infrared spectrum of 3,5-di-tert-butyl salicylaldehyde in the example of the present invention;
[0036] Figure 2 This is an infrared spectrum of the L-lysine Schiff base zinc complex prepared in Example 1 of the present invention;
[0037] Figure 3 This is an infrared spectrum of the L-histidine Schiff base zinc complex prepared in Example 2 of the present invention;
[0038] Figure 4 This is the infrared spectrum of the L-arginine Schiff base zinc complex prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0039] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0040] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.
[0041] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.
[0042] Example 1 Preparation of safe and non-toxic medical polymer catalyst: lysine Schiff base zinc complex
[0043] Weigh 10mmol L-lysine (1.4619g) in a three-necked flask, add 30mL of anhydrous methanol, then add 10mmol of potassium hydroxide (0.5611g), start magnetic stirring at 25℃ for 10min, and obtain a white suspension. Then gradually add 20mL of anhydrous methanol solution containing 10mmol 3,5-di-tert-butyl salicylaldehyde (2.3433g) to the solution, and the solution gradually turns light yellow. After the addition is complete, heat to 60℃ and reflux for 3h. It can be found through the TCL point plate that 3,5-di-tert-butyl salicylaldehyde has basically reacted, and then continue to add 10mmol of zinc acetate (1.2543g). After the addition is complete, continue to reflux at 60℃ for 3h. After the reaction is completed, cool naturally to room temperature, and let it stand in the refrigerator overnight. A yellow solid precipitates. Filter and collect the precipitate to obtain lysine Schiff base zinc complex with a yield of 42%.
[0044] Example 2 Preparation of safe and non-toxic medical polymer catalyst: Histidine Schiff base zinc complex
[0045] Weigh 10mmol L-histidine (1.5516g) in a three-necked flask, add 30mL of anhydrous methanol, then add 10mmol of potassium hydroxide (0.5611g), start magnetic stirring at 25℃ for 10min, and obtain a white suspension. Then gradually add 20mL of anhydrous methanol solution containing 10mmol 3,5-di-tert-butyl salicylaldehyde (2.3433g) to the solution, and the solution gradually turns light yellow. After the addition is complete, heat to 60℃ and reflux for 3h. It can be found through the TCL point plate that 3,5-di-tert-butyl salicylaldehyde has basically reacted, and then continue to add 10mmol of zinc acetate (1.2543g). After the addition is complete, continue to reflux at 60℃ for 3h. After the reaction is completed, cool naturally to room temperature, and let it stand in the refrigerator overnight. A light yellow solid precipitates. Filter and collect the precipitate to obtain histidine Schiff base zinc complex with a yield of 53%.
[0046] Example 3 Preparation of safe and non-toxic medical polymer catalyst: Arginine Schiff base zinc complex
[0047] Weigh 10mmol L-arginine (1.5516g) in a three-necked flask, add 30mL of anhydrous methanol, then add 10mmol of potassium hydroxide (0.5611g), start magnetic stirring at 25℃ for 10min, and obtain a white suspension. Then gradually add 20mL of anhydrous methanol solution containing 10mmol of 3,5-di-tert-butyl salicylaldehyde (2.3433g) to the solution, and the solution gradually turns light yellow. After the addition is complete, heat to 60℃ and reflux for 3h. It can be found through the TCL point plate that 3,5-di-tert-butyl salicylaldehyde has basically reacted, and then continue to add 10mmol of zinc acetate (1.2543g). After the addition is complete, continue to reflux at 60℃ for 3h. After the reaction is completed, cool naturally to room temperature, and let it stand in the refrigerator overnight. A brown-red solid precipitates. Filter and collect the precipitate to obtain arginine Schiff base zinc complex with a yield of 78%.
[0048] Furthermore, 3,5-di-tert-butyl salicylaldehyde was tested by infrared spectroscopy analysis to facilitate the comparison of the functional group structure with the synthesized amino acid Schiff base zinc complex. Figure 1 As shown, at 1391.67cm -1 and 1363.58cm -1 The two absorption peaks are characteristic absorption peaks of tert-butyl. -1 There is an absorption peak nearby, which is the stretching vibration absorption of the benzene ring Ar-H, at 881.24cm -1 There is a strong absorption peak nearby, which corresponds to the out-of-plane bending vibration absorption peak of the tetrasubstituted 1,2,3,5-carbon-hydrogen bonds of the benzene ring, thereby determining the position of the absorption peak of the key functional group of 3,5-di-tert-butyl salicylaldehyde.
[0049] The lysine Schiff base zinc complex synthesized in Example 1 was tested by infrared spectroscopy analysis ( Figure 2 ),like Figure 2 As shown, at 3420.20cm -1 There is a strong and broad peak at 770.54 cm-1, which is attributed to the absorption peak of -NH2 on the crystal water or lysine. -1 and 711.37cm -1 There is an absorption peak, which is caused by the bending vibration of CH on the benzene ring, indicating that there is a benzene ring structure in the product. -1 There is a strong absorption peak, which is caused by the stretching vibration of -C=N-, indicating that the amino acid and 3,5-di-tert-butyl salicylaldehyde undergo a condensation reaction to produce an imine bond and introduce a benzene ring structure and a carbon-carbon double bond. In addition, at 643.64 cm -1 and 771.37cm -1 A new strong absorption peak (674.13 cm-1 ), corresponding to the metal ion absorption peak, indicating the successful synthesis of lysine Schiff base zinc complex.
[0050] The histidine Schiff base zinc complex synthesized in Example 2 was tested by infrared spectroscopy analysis ( Figure 3 ),like Figure 3 As shown, at 3413.51cm -1 There is a strong and broad peak at 770.02 cm -1 and 746.47cm -1 The absorption peak at 1621.61cm is the bending vibration of CH on the benzene ring, indicating the presence of a benzene ring structure in the product. -1 The strong absorption peak at 617.99 cm -1 and 746.47cm -1 The strong absorption peak that appears between them corresponds to the coordination peak of zinc metal ions. The above results characterize the successful preparation of the histidine Schiff base zinc complex.
[0051] The arginine Schiff base zinc complex synthesized in Example 3 was tested by infrared spectroscopy analysis ( Figure 4 ),like Figure 4 As shown, at 3360.05cm -1 There is a broad peak at 770.02 and 712.33, which is attributed to the absorption peak of -NH2 on the crystal water or arginine. The absorption peaks at 1392.04 cm -1 and 1361.50cm -1 For the two characteristic peaks of tert-butyl, further, 1621.51 cm -1 There is a strong absorption peak corresponding to the stretching vibration of -C=N-, and at 615.99 cm -1 and 712.33cm -1 The strong absorption peak (672.25cm -1 ) corresponds to the zinc metal ion peak, thus confirming the successful synthesis of the arginine Schiff base zinc complex.
[0052] Example 4 Application of the catalyst obtained in Example 1 in the polycondensation reaction of lactide and glycolide to synthesize poly(lactide-glycolide) copolymer
[0053] Under anhydrous and oxygen-free conditions, 36 mmol of recrystallized left-lactide (L-LA) and 4 mmol of recrystallized glycolide (GA) were mixed, and 0.04 mmol of the lysine Schiff base zinc catalyst obtained in Example 1 was added and mixed, and the mixture was first vacuumed at 65° C. for 1 h, and then the temperature was raised to 135-140° C. and stirred for reaction for 1 h. 30 mL of dichloromethane was added to the obtained reaction product to dissolve the polymer, and then an excess of ethanol was added thereto to precipitate the polymer, and the mixture was filtered and vacuum dried for 48 h to obtain poly(lactide-glycolide) (L-LA:GA=90:10).
[0054] The weight of the poly(lactide) obtained by the present invention is 4.7 g, and the yield is 90%. The poly(lactide) copolymer obtained in this embodiment is analyzed by gel permeation chromatography using polystyrene as a standard, and the number average molecular weight of the poly(lactide) is 1.8w, and Pm=1.56.
[0055] Example 5 Application of the catalyst obtained in Example 1 in the polycondensation reaction of lactide and glycolide to synthesize poly(lactide-glycolide) copolymer
[0056] Under anhydrous and oxygen-free conditions, 36 mmol of recrystallized L-lactide and 4 mmol of recrystallized glycolide were mixed, and 0.04 mmol of the lysine Schiff base zinc catalyst obtained in Example 1 was added and mixed. The mixture was first vacuumed at 65° C. for 1 h, then heated to 170-175° C. and stirred for reaction for 8 h. 30 mL of dichloromethane was added to the obtained reaction product to dissolve the polymer, and then an excess of ethanol was added thereto to precipitate the polymer. The mixture was filtered and vacuum dried for 48 h to obtain poly(lactide-glycolide).
[0057] The weight of the poly(lactide) obtained by the present invention is 4.8 g, and the yield is 93%. The poly(lactide) obtained by the present invention is analyzed by gel permeation chromatography using polystyrene as a standard, and the number average molecular weight of the poly(lactide) is 87,000, and Pm=1.52.
[0058] Example 6 Application of the catalyst obtained in Example 1 in the polycondensation reaction of lactide and glycolide to synthesize poly(lactide-glycolide) copolymer
[0059] Under anhydrous and oxygen-free conditions, 36 mmol of recrystallized L-lactide and 4 mmol of recrystallized glycolide were mixed, and 0.04 mmol of the lysine Schiff base zinc catalyst obtained in Example 1 was added and mixed. The mixture was first vacuumed at 65° C. for 1 h, then heated to 170-175° C. and stirred for reaction for 16 h. 30 mL of dichloromethane was added to the obtained reaction product to dissolve the polymer, and then an excess of ethanol was added thereto to precipitate the polymer. The mixture was filtered and vacuum dried for 48 h to obtain poly(lactide-glycolide).
[0060] The weight of the poly(lactide) obtained by the present invention is 4.8 g, and the yield is 93%. The poly(lactide) copolymer obtained in this embodiment is analyzed by gel permeation chromatography using polystyrene as a standard, and the number average molecular weight of the poly(lactide) is 7.6w, and Pm=1.63.
[0061] Example 7 Application of the catalyst obtained in Example 1 in the polycondensation reaction of lactide and glycolide to synthesize poly(lactide-glycolide) copolymer
[0062] Under anhydrous and oxygen-free conditions, 36 mmol of recrystallized L-lactide and 4 mmol of recrystallized glycolide were mixed, and 0.04 mmol of the lysine Schiff base zinc catalyst obtained in Example 1 was added and mixed. The mixture was first vacuumed at 65° C. for 1 h, then heated to 140-145° C. and stirred for reaction for 8 h. 30 mL of dichloromethane was added to the obtained reaction product to dissolve the polymer, and then an excess of ethanol was added thereto to precipitate the polymer. The mixture was filtered and vacuum dried for 48 h to obtain poly(lactide-glycolide).
[0063] The weight of the poly(lactide) obtained by the present invention is 4.8 g, and the yield is 92%. The poly(lactide) obtained by the present invention is analyzed by gel permeation chromatography using polystyrene as a standard, and the number average molecular weight of the poly(lactide) is 68,000, and Pm=1.56.
[0064] Example 8 Application of the catalyst obtained in Example 1 in the polycondensation reaction of lactide and glycolide to synthesize poly(lactide-glycolide) copolymer
[0065] Under anhydrous and oxygen-free conditions, 36 mmol of recrystallized L-lactide and 4 mmol of recrystallized glycolide were mixed, and 0.04 mmol of the lysine Schiff base zinc catalyst obtained in Example 1 was added and mixed. The mixture was first vacuumed at 65° C. for 1 h, then heated to 190-195° C. and stirred for reaction for 8 h. 30 mL of dichloromethane was added to the obtained reaction product to dissolve the polymer, and then an excess of ethanol was added thereto to precipitate the polymer. The mixture was filtered and vacuum dried for 48 h to obtain poly(lactide-glycolide).
[0066] The weight of the poly(lactide) obtained by the present invention is 4.8 g, and the yield is 92%. The poly(lactide) copolymer obtained in this embodiment is analyzed by gel permeation chromatography using polystyrene as a standard, and the number average molecular weight of the poly(lactide) is 7.3w, and Pm=1.64.
[0067] Table 1 Comparison of reaction parameters and results of Examples 4-8
[0068] Monomer: Catalyst Reaction time / h Reaction temperature / ℃ Yield Number average molecular weight Pm Example 4 500:1 1 170-175 90% 1.8w 1.56 Example 5 500:1 8 170-175 93% 8.7w 1.52 Example 6 500:1 16 170-175 92% 7.6w 1.63 Example 7 500:1 8 140~145 92% 5.3w 1.56 Example 8 500:1 8 190-195 92% 6.4w 1.64
[0069] Example 9 Application of the catalyst obtained in Example 2 in the polycondensation reaction of lactide and glycolide to synthesize poly(lactide-glycolide) copolymer
[0070] Under anhydrous and oxygen-free conditions, 36 mmol of recrystallized L-lactide and 4 mmol of recrystallized glycolide were mixed, and 0.04 mmol of the histidine Schiff base zinc catalyst obtained in Example 2 was added and mixed, and the mixture was first vacuumed at 65° C. for 1 h, and then the temperature was raised to 170-175° C. and stirred for reaction for 1 h. 30 mL of dichloromethane was added to the obtained reaction product to dissolve the polymer, and then an excess of ethanol was added thereto to precipitate the polymer, filtered, and vacuum dried for 48 h to obtain poly(lactide-glycolide) (L-LA:GA=90:10).
[0071] The weight of the poly(lactide) obtained by the present invention is 4.5 g, and the yield is 87%. The poly(lactide) copolymer obtained in this embodiment is analyzed by gel permeation chromatography using polystyrene as a standard, and the number average molecular weight of the poly(lactide) is 1.2w, and Pm=1.64.
[0072] Example 10 Application of the catalyst obtained in Example 2 in the polycondensation reaction of lactide and glycolide to synthesize poly(lactide-glycolide) copolymer
[0073] Under anhydrous and oxygen-free conditions, 36 mmol of recrystallized L-lactide and 4 mmol of recrystallized glycolide were mixed, and 0.04 mmol of the histidine Schiff base zinc catalyst obtained in Example 2 was added and mixed, and the mixture was first vacuumed at 65° C. for 1 h, and then the temperature was raised to 170-175° C. and stirred for reaction for 8 h. 30 mL of dichloromethane was added to the obtained reaction product to dissolve the polymer, and then an excess of ethanol was added thereto to precipitate the polymer, and the mixture was filtered and vacuum dried for 48 h to obtain poly(lactide-glycolide).
[0074] The weight of the poly(lactide) obtained by the present invention is 4.6 g, and the yield is 88%. The poly(lactide) copolymer obtained in this embodiment is analyzed by gel permeation chromatography using polystyrene as a standard, and the number average molecular weight of the poly(lactide) is 6.8w, and Pm=1.64.
[0075] Example 11 Application of the catalyst obtained in Example 2 in the polycondensation reaction of lactide and glycolide to synthesize poly(lactide-glycolide) copolymer
[0076] Under anhydrous and oxygen-free conditions, 36 mmol of recrystallized L-lactide and 4 mmol of recrystallized glycolide were mixed, and 0.04 mmol of the histidine Schiff base zinc catalyst obtained in Example 2 was added and mixed, and the mixture was first vacuumed at 65° C. for 1 h, and then the temperature was raised to 170-175° C. and stirred for reaction for 12 h. 30 mL of dichloromethane was added to the obtained reaction product to dissolve the polymer, and then an excess of ethanol was added thereto to precipitate the polymer, and the mixture was filtered and vacuum dried for 48 h to obtain poly(lactide-glycolide).
[0077] The weight of the poly(lactide) obtained by the present invention is 4.3 g, and the yield is 83%. The poly(lactide) copolymer obtained in this embodiment is analyzed by gel permeation chromatography using polystyrene as a standard, and the number average molecular weight of the poly(lactide) is 5.4w, and Pm=1.68.
[0078] Example 12 Application of the catalyst obtained in Example 2 in the polycondensation reaction of lactide and glycolide to synthesize poly(lactide-glycolide) copolymer
[0079] Under anhydrous and oxygen-free conditions, 36 mmol of recrystallized L-lactide and 4 mmol of recrystallized glycolide were mixed, and 0.04 mmol of the histidine Schiff base zinc catalyst obtained in Example 2 was added and mixed, and the mixture was first vacuumed at 65° C. for 1 h, and then the temperature was raised to 140-145° C. and stirred for reaction for 8 h. 30 mL of dichloromethane was added to the obtained reaction product to dissolve the polymer, and then an excess of ethanol was added thereto to precipitate the polymer, filtered, and vacuum dried for 48 h to obtain poly(lactide-glycolide).
[0080] The weight of the poly(lactide) obtained by the present invention is 4.3 g, and the yield is 83%. The poly(lactide) copolymer obtained in this embodiment is analyzed by gel permeation chromatography using polystyrene as a standard, and the number average molecular weight of the poly(lactide) is 5.8w, and Pm=1.60.
[0081] Example 13 Application of the catalyst obtained in Example 2 in the polycondensation reaction of lactide and glycolide to synthesize poly(lactide-glycolide) copolymer
[0082] Under anhydrous and oxygen-free conditions, 36 mmol of recrystallized L-lactide and 4 mmol of recrystallized glycolide were mixed, and 0.04 mmol of the histidine Schiff base zinc catalyst obtained in Example 2 was added and mixed, and the mixture was first vacuumed at 65° C. for 1 h, and then the temperature was raised to 190-195° C. and stirred for reaction for 8 h. 30 mL of dichloromethane was added to the obtained reaction product to dissolve the polymer, and then an excess of ethanol was added thereto to precipitate the polymer, filtered, and vacuum dried for 48 h to obtain poly(lactide-glycolide) (L-LA:GA=1:1).
[0083] The weight of the poly(lactide) obtained by the present invention is 4.4 g, and the yield is 85%. The poly(lactide) copolymer obtained in this embodiment is analyzed by gel permeation chromatography using polystyrene as a standard, and the number average molecular weight of the poly(lactide) is 5.7w, and Pm=1.62.
[0084] Table 2 Comparison of reaction parameters and results of Examples 9-13
[0085]
[0086]
[0087] Example 14 Application of the catalyst obtained in Example 3 in the polycondensation reaction of lactide and glycolide to synthesize poly(lactide-glycolide) copolymer
[0088] Under anhydrous and oxygen-free conditions, 36 mmol of recrystallized L-lactide and 4 mmol of recrystallized glycolide were mixed, and 0.04 mmol of the arginine Schiff base zinc catalyst obtained in Example 3 was added and mixed, and the mixture was first vacuumed at 65° C. for 1 h, and then the temperature was raised to 170-175° C. and stirred for reaction for 1 h. 30 mL of dichloromethane was added to the obtained reaction product to dissolve the polymer, and then an excess of ethanol was added thereto to precipitate the polymer, filtered, and vacuum dried for 48 h to obtain poly(lactide-glycolide) (L-LA:GA=90:10).
[0089] The weight of the poly(lactide) obtained by the present invention is 4.4 g, and the yield is 85%. The poly(lactide) copolymer obtained in this embodiment is analyzed by gel permeation chromatography using polystyrene as a standard, and the number average molecular weight of the poly(lactide) is 0.87w, and Pm=1.58.
[0090] Example 15 Application of the catalyst obtained in Example 3 in the polycondensation reaction of lactide and glycolide to synthesize poly(lactide-glycolide) copolymer
[0091] Under anhydrous and oxygen-free conditions, 36 mmol of recrystallized L-lactide and 4 mmol of recrystallized glycolide were mixed, and 0.04 mmol of the arginine Schiff base zinc catalyst obtained in Example 3 was added and mixed, and the mixture was first vacuumed at 65° C. for 1 h, and then the temperature was raised to 170-175° C. and stirred for reaction for 8 h. 30 mL of dichloromethane was added to the obtained reaction product to dissolve the polymer, and then an excess of ethanol was added thereto to precipitate the polymer, and the mixture was filtered and vacuum dried for 48 h to obtain poly(lactide-glycolide).
[0092] The weight of the poly(lactide) obtained by the present invention is 4.2 g, and the yield is 81%. The poly(lactide) copolymer obtained in this embodiment is analyzed by gel permeation chromatography using polystyrene as a standard, and the number average molecular weight of the poly(lactide) is 4.3w, and Pm=1.63.
[0093] Example 16 Application of the catalyst obtained in Example 3 in the polycondensation reaction of lactide and glycolide to synthesize poly(lactide-glycolide) copolymer
[0094] Under anhydrous and oxygen-free conditions, 36 mmol of recrystallized L-lactide and 4 mmol of recrystallized glycolide were mixed, and 0.04 mmol of the arginine Schiff base zinc catalyst obtained in Example 3 was added and mixed, and the mixture was first vacuumed at 65° C. for 1 h, and then the temperature was raised to 170-175° C. and stirred for reaction for 12 h. 30 mL of dichloromethane was added to the obtained reaction product to dissolve the polymer, and then an excess of ethanol was added thereto to precipitate the polymer, and the mixture was filtered and vacuum dried for 48 h to obtain poly(lactide-glycolide).
[0095] The weight of the poly(lactide) obtained by the present invention is 4.5 g, and the yield is 87%. The poly(lactide) copolymer obtained in this embodiment is analyzed by gel permeation chromatography using polystyrene as a standard, and the number average molecular weight of the poly(lactide) is 3.8w, and Pm=1.64.
[0096] Example 17 Application of the catalyst obtained in Example 3 in the polycondensation reaction of lactide and glycolide to synthesize poly(lactide-glycolide) copolymer
[0097] Under anhydrous and oxygen-free conditions, 36 mmol of recrystallized L-lactide and 4 mmol of recrystallized glycolide were mixed, and 0.04 mmol of the arginine Schiff base zinc catalyst obtained in Example 3 was added and mixed, and the mixture was first vacuumed at 65° C. for 1 h, and then the temperature was raised to 140-145° C. and stirred for reaction for 8 h. 30 mL of dichloromethane was added to the obtained reaction product to dissolve the polymer, and then an excess of ethanol was added thereto to precipitate the polymer, and the mixture was filtered and vacuum dried for 48 h to obtain poly(lactide-glycolide).
[0098] The weight of the poly(lactide) obtained by the present invention is 4.3 g, and the yield is 83%. The poly(lactide) copolymer obtained in this embodiment is analyzed by gel permeation chromatography using polystyrene as a standard, and the number average molecular weight of the poly(lactide) is 3.9w, and Pm=1.61.
[0099] Example 18 Application of the catalyst obtained in Example 3 in the polycondensation reaction of lactide and glycolide to synthesize poly(lactide-glycolide) copolymer
[0100] Under anhydrous and oxygen-free conditions, 36 mmol of recrystallized L-lactide and 4 mmol of recrystallized glycolide were mixed, and 0.04 mmol of the arginine Schiff base zinc catalyst obtained in Example 3 was added and mixed, and the mixture was first vacuumed at 65° C. for 1 h, and then the temperature was raised to 190-195° C. and stirred for reaction for 8 h. 30 mL of dichloromethane was added to the obtained reaction product to dissolve the polymer, and then an excess of ethanol was added thereto to precipitate the polymer, and the mixture was filtered and vacuum dried for 48 h to obtain poly(lactide-glycolide).
[0101] The weight of the poly(lactide) obtained by the present invention is 4.4 g, and the yield is 84%. The poly(lactide) copolymer obtained in this embodiment is analyzed by gel permeation chromatography using polystyrene as a standard, and the number average molecular weight of the poly(lactide) is 3.1w, and Pm=1.68.
[0102] Table 3 Comparison of reaction parameters and results of Examples 14-18
[0103] Monomer: Catalyst Reaction time / h Reaction temperature / ℃ Yield Number average molecular weight Pm Embodiment 14 500:1 1 170-175 85% 0.87w 1.58 Embodiment 15 500:1 8 170-175 81% 4.3w 1.63 Example 16 500:1 16 170-175 87% 3.8w 1.64 Embodiment 17 500:1 8 140~145 83% 3.9w 1.61 Embodiment 18 500:1 8 190-195 84% 3.1w 1.68
[0104] Furthermore, setting other reaction conditions to be the same, the lysine Schiff base zinc catalyst prepared in Example 1 was used to study the effect of the ratio of lactide to glycolide on the molecular weight of the copolymer under preferred conditions.
[0105] Example 19 Application of the catalyst obtained in Example 1 in the polycondensation reaction of lactide and glycolide to synthesize poly(lactide-glycolide) copolymer (optimized conditions)
[0106] Under anhydrous and oxygen-free conditions, 32 mmol of recrystallized L-lactide and 8 mmol of recrystallized glycolide were mixed, and 0.04 mmol of the lysine Schiff base zinc catalyst obtained in Example 1 was added and mixed, and the mixture was first vacuumed at 65° C. for 1 h, and then the temperature was raised to 170-175° C. and stirred for reaction for 8 h. 30 mL of dichloromethane was added to the obtained reaction product to dissolve the polymer, and then an excess of ethanol was added thereto to precipitate the polymer, filtered, and vacuum dried for 48 h to obtain poly(lactide-glycolide) (L-LA:GA=80:20).
[0107] The weight of the poly(lactide) obtained by the present invention is 5.1 g, and the yield is 92%. The poly(lactide) copolymer obtained in this embodiment is analyzed by gel permeation chromatography using polystyrene as a standard, and the number average molecular weight of the poly(lactide) is 7.6w, and Pm=1.56.
[0108] Example 20 Application of the catalyst obtained in Example 1 in the polycondensation reaction of lactide and glycolide to synthesize poly(lactide-glycolide) copolymer (optimized conditions)
[0109] Under anhydrous and oxygen-free conditions, 30 mmol of recrystallized L-lactide and 10 mmol of recrystallized glycolide were mixed, and 0.04 mmol of the lysine Schiff base zinc catalyst obtained in Example 1 was added and mixed, and the mixture was first vacuumed at 65° C. for 1 h, and then the temperature was raised to 170-175° C. and stirred for reaction for 8 h. 30 mL of dichloromethane was added to the obtained reaction product to dissolve the polymer, and then an excess of ethanol was added thereto to precipitate the polymer, filtered, and vacuum dried for 48 h to obtain poly(lactide-glycolide) (L-LA:GA=75:25).
[0110] The weight of the poly(lactide) obtained by the present invention is 4.9 g, and the yield is 90%. The poly(lactide) copolymer obtained in this embodiment is analyzed by gel permeation chromatography using polystyrene as a standard, and the number average molecular weight of the poly(lactide) is 7.3w, and Pm=1.57.
[0111] Example 21 Application of the catalyst obtained in Example 1 in the polycondensation reaction of lactide and glycolide to synthesize poly(lactide-glycolide) copolymer (optimized conditions)
[0112] Under anhydrous and oxygen-free conditions, 28 mmol of recrystallized L-lactide and 12 mmol of recrystallized glycolide were mixed, and 0.04 mmol of the lysine Schiff base zinc catalyst obtained in Example 1 was added and mixed, and the mixture was first vacuumed at 65° C. for 1 h, and then the temperature was raised to 170-175° C. and stirred for reaction for 8 h. 30 mL of dichloromethane was added to the obtained reaction product to dissolve the polymer, and then an excess of ethanol was added thereto to precipitate the polymer, filtered, and vacuum dried for 48 h to obtain poly(lactide-glycolide) (L-LA:GA=70:20).
[0113] The weight of the poly(lactide) obtained by the present invention is 5.0 g, and the yield is 93%. The poly(lactide) copolymer obtained in this embodiment is analyzed by gel permeation chromatography using polystyrene as a standard, and the number average molecular weight of the poly(lactide) is 7.2w, and Pm=1.55.
[0114] Example 22 Application of the catalyst obtained in Example 1 in the polycondensation reaction of lactide and glycolide to synthesize poly(lactide-glycolide) copolymer (optimized conditions)
[0115] Under anhydrous and oxygen-free conditions, 24 mmol of recrystallized L-lactide and 16 mmol of recrystallized glycolide were mixed, and 0.04 mmol of the lysine Schiff base zinc catalyst obtained in Example 1 was added and mixed, and the mixture was first vacuumed at 65° C. for 1 h, and then the temperature was raised to 170-175° C. and stirred for reaction for 8 h. 30 mL of dichloromethane was added to the obtained reaction product to dissolve the polymer, and then an excess of ethanol was added thereto to precipitate the polymer, and the mixture was filtered and vacuum dried for 48 h to obtain poly(lactide-glycolide) (L-LA:GA=60:40).
[0116] The weight of the poly(lactide) obtained by the present invention is 4.8 g, and the yield is 91%. The poly(lactide) copolymer obtained in this embodiment is analyzed by gel permeation chromatography using polystyrene as a standard, and the number average molecular weight of the poly(lactide) is 6.7w, and Pm=1.54.
[0117] Example 23 Application of the catalyst obtained in Example 1 in the polycondensation reaction of lactide and glycolide to synthesize poly(lactide-glycolide) copolymer (optimized conditions)
[0118] Under anhydrous and oxygen-free conditions, 20 mmol of recrystallized L-lactide and 20 mmol of recrystallized glycolide were mixed, and 0.04 mmol of the lysine Schiff base zinc catalyst obtained in Example 1 was added and mixed, and the mixture was first vacuumed at 65° C. for 1 h, and then the temperature was raised to 170-175° C. and stirred for reaction for 8 h. 30 mL of dichloromethane was added to the obtained reaction product to dissolve the polymer, and then an excess of ethanol was added thereto to precipitate the polymer, and the mixture was filtered and vacuum dried for 48 h to obtain poly(lactide-glycolide) (L-LA:GA=50:50).
[0119] The weight of the poly(lactide) obtained by the present invention is 4.6 g, and the yield is 88%. The poly(lactide) copolymer obtained in this embodiment is analyzed by gel permeation chromatography using polystyrene as a standard, and the number average molecular weight of the poly(lactide) is 5.6w, and Pm=1.55.
[0120] Table 4 Comparison of reaction parameters and results of Example 5 and Examples 19-22
[0121] L-LA:GA Reaction time / h Reaction temperature / ℃ Yield Number average molecular weight Pm Example 5 90:10 8 170-175 93% 8.7w 1.52 Embodiment 19 80:20 8 170-175 92% 7.6w 1.56 Embodiment 20 75:25 8 170-175 90% 7.3w 1.57 Embodiment 21 70:30 8 170-175 93% 7.2w 1.55 Embodiment 22 60:40 8 170-175 91% 6.7w 1.54 Embodiment 22 50:50 8 170-175 88% 5.6w 1.55
[0122] It can be seen from the above examples that the present invention provides an amino acid Schiff base zinc complex catalyst and a preparation method thereof, and the obtained catalyst can indeed be used as a catalyst in the synthesis of poly(lactide-co-glycolide), and can achieve the purpose of the invention.
[0123] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
[0124] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.
Claims
1. A safe and non-toxic medical polymer catalyst, characterized in that: The catalyst is an amino acid Schiff base zinc complex, and the amino acid includes one or more of lysine, histidine and arginine.
2. The safe and nontoxic medical polymer catalyst according to claim 1, characterized in that: The amino acid Schiff base zinc complex has the following structures: Among them, formula (1) is a lysine Schiff base zinc complex, formula (2) is a histidine Schiff base zinc complex, and formula (3) is an arginine Schiff base zinc complex.
3. A method for preparing the safe and nontoxic medical polymer catalyst according to claim 1 or 2, characterized in that: The following steps are involved: (1) adding an amino acid and an inorganic base into a solvent, mixing and stirring, and then adding 3,5-di-tert-butyl salicylaldehyde to carry out a nucleophilic addition reaction to obtain an amino acid Schiff base complex containing an imine group; (2) Adding zinc acetate to the product obtained in step (1) to continue the reaction, cooling after the reaction is completed, recrystallizing under low temperature conditions, separating the product, and obtaining a solid powder, which is an amino acid Schiff base zinc complex.
4. The method for preparing a safe and nontoxic medical polymer catalyst according to claim 3, characterized in that: The molar ratio of the amino acid to the inorganic base in step (1) is 1:(1.0-1.4).
5. The method for preparing a safe and nontoxic medical polymer catalyst according to claim 3, characterized in that: The molar ratio of the amino acid to 3,5-di-tert-butyl salicylaldehyde in step (1) is 1:(1.0-1.5).
6. The method for preparing a safe and nontoxic medical polymer catalyst according to claim 3, characterized in that: The molar ratio of the zinc acetate in step (2) to the amino acid bound in the product of step (1) is (1.0-2.0):
1.
7. The method for preparing a safe and nontoxic medical polymer catalyst according to claim 3, characterized in that: The ratio of the amount of the amino acid in step (1) to the volume of the solvent is (0.01-0.015) mol:50 mL.
8. The method for preparing a safe and nontoxic medical polymer catalyst according to claim 3, characterized in that: In step (1), the stirring temperature is 20-30° C., the stirring time is 10-30 min, the nucleophilic addition reaction temperature is 55-60° C., and the reaction time is 2-4 h.
9. The method for preparing a safe and nontoxic medical polymer catalyst according to claim 3, characterized in that:
3. The reaction temperature of step (2) is 55-60° C. and the reaction time is 3-5 h.
10. Use of the safe and non-toxic medical polymer catalyst according to claim 1 or 2 as a catalyst in a ring-opening polymerization reaction.