Preparation method and application of polyether polyol for adhesive

The method for preparing polyether polyols and adhesives by autocatalysis solves the problems of cumbersome preparation processes and insufficient performance of existing adhesives, and achieves low cost, high water and air permeability and excellent mechanical properties.

CN118909239APending Publication Date: 2024-11-08JIANGSU ZHONGSHAN NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411048166.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing adhesives have complicated preparation processes, high costs, and insufficient mechanical and environmental performance.

Method used

A self-catalytic preparation method is adopted, in which amine compounds and epoxides are added to a polymerization reactor to prepare polyether polyols, which are then reacted with polymethylene polyphenyl isocyanate, crosslinking agents and thixotropic agents to prepare adhesives, thus avoiding the use of catalysts.

Benefits of technology

It achieves low cost, high water and air permeability, and excellent mechanical properties, while meeting environmental protection requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004974094170000071
    Figure BDA0004974094170000071
Patent Text Reader

Abstract

The invention provides a preparation method and application of polyether polyol for an adhesive, and relates to the field of organic synthesis. The preparation method comprises the following steps: (1) adding an amine compound into a polymerization reaction kettle, carrying out nitrogen replacement, heating to 90-130 DEG C, and carrying out heat preservation; (2) introducing an epoxide, and carrying out a reaction at 90-120 DEG C; and (3) when the pressure in the kettle is reduced to negative pressure, cooling to 90-110 DEG C, vacuumizing, and then cooling to room temperature to obtain the polyether polyol for the adhesive. The polyether polyol for the adhesive prepared by the method is simple in production process, self-catalyzed and low in cost, and the adhesive prepared from the polyether polyol is excellent in mechanical property, environment-friendly and high in moisture permeability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of organic synthesis, and in particular to a preparation method of polyether polyol for adhesive and application thereof. Background Art

[0002] Adhesives are widely used in sports facilities, medical equipment, auto parts, transportation, building materials, etc. In the prior art, the preparation of polyether polyols for adhesives requires the use of catalysts, which are then removed through post-processing. The production cost is high and the process is complicated. In addition, the mechanical properties of existing adhesives cannot meet actual needs and do not meet environmental protection requirements. Summary of the invention

[0003] In order to solve the above-mentioned shortcomings, the present invention provides a method for preparing polyether polyol for adhesive, which has simple production process, self-catalysis and low cost. The adhesive prepared by using the polyether polyol has excellent mechanical properties, is environmentally friendly, and has high water vapor permeability.

[0004] The purpose of the present invention is achieved by the following technical solutions:

[0005] A method for preparing a polyether polyol for an adhesive comprises the following steps:

[0006] (1) Adding an amine compound into a polymerization reaction kettle, replacing the atmosphere with nitrogen, and heating the reactor to 90-130° C. and keeping the temperature constant;

[0007] (2) introducing epoxide and reacting at 90° C. to 120° C.;

[0008] (3) When the pressure in the autoclave is reduced to negative pressure, the temperature is lowered to 90-110° C., vacuumized, and then lowered to room temperature to obtain the polyether polyol for the adhesive.

[0009] In the present invention, the amine compound is aniline.

[0010] In the present invention, the epoxide is a mixture of ethylene oxide and butylene oxide.

[0011] In the present invention, the molar ratio of the epoxide to the amine compound is 1-2.5:1.

[0012] In the present invention, the mass of ethylene oxide in the epoxide accounts for 1% to 50% of the total mass of ethylene oxide and butylene oxide; in the preferred technical solution, the mass of ethylene oxide in the epoxide accounts for 9% to 12% of the total mass of ethylene oxide and butylene oxide.

[0013] In the present invention, in step (2), a portion of the epoxide is first introduced to induce the reaction, and then the remaining portion of the epoxide is introduced, and the mass ratio of the epoxide introduced twice is 1:13-15.

[0014] In the present invention, the number average molecular weight of the polyether polyol for adhesive is 200-500 Daltons.

[0015] The present invention also provides a method for preparing an adhesive, comprising the following steps:

[0016] (1) vacuum dehydrating the polyether polyol prepared by the method;

[0017] (2) heating 70-90 parts by weight of polymethylene polyphenyl isocyanate to 42-48° C., then dripping 90-110 parts by weight of the dehydrated polyether polyol described in step (1), reacting at 42-48° C. for 0.3-0.7 hours, dripping 4-6 parts by weight of a crosslinking agent, and continuing to react at 42-48° C. for 0.8-1.2 hours;

[0018] (3) raising the temperature to 48-52° C., adding 0.4-0.6 parts by weight of a catalyst and 1.3-1.7 parts by weight of a thixotropic agent, reacting for 20-40 minutes, and cooling to room temperature to obtain the adhesive.

[0019] In the present invention, the crosslinking agent is ethylene glycol, the catalyst is dibutyltin dilaurate, the thixotropic agent is fumed silica, and the polymethylene polyphenyl isocyanate is a mixture of toluene diisocyanate and diphenylmethane diisocyanate in a mass ratio of 1:1.

[0020] The method of the invention prepares a polyether polyol for an adhesive, does not require any catalyst in the synthesis reaction process, has simple production process, low cost, excellent mechanical properties, is environmentally friendly, and has high water vapor permeability. DETAILED DESCRIPTION

[0021] The following examples will further illustrate the synthesis method of the invention, but the present invention is not limited to the listed examples, but should also include other known changes within the scope of the claims.

[0022] Example 1 Synthesis of polyether polyols a, b and c

[0023] 1. Synthesizing polyether polyol a, comprising the following steps:

[0024] (1) 233 g of aniline (Shandong Qixing Chemical Co., Ltd.) was added to a 1 L polymerization reactor at room temperature. After nitrogen replacement, the vacuum was turned off. At this time, the pressure in the reactor was -0.1 MPa; the temperature was raised to 110°C.

[0025] (2) First, a mixture of 5 g of ethylene oxide and 45 g of butylene oxide was introduced to raise the pressure in the autoclave to 0.35 MPa for induction reaction. When the pressure in the autoclave slowly decreased and the temperature gradually increased, it indicated that the induced reaction was successful. Then, a mixture of 71.7 g of ethylene oxide and 645.3 g of butylene oxide was continuously introduced. During the continuous introduction of the mixture of ethylene oxide and butylene oxide, the pressure in the autoclave was controlled to be 0.2 MPa and the temperature in the autoclave was controlled to be 110°C.

[0026] (3) After continuously introducing a mixture of ethylene oxide and butylene oxide, the reaction was carried out at 110°C. When the pressure in the autoclave dropped to -0.1 MPa, the reaction was terminated, the temperature was lowered to 100°C, and vacuum was drawn for 1 hour. Finally, the temperature was lowered to room temperature and the material was discharged to obtain polyether polyol a. The hydroxyl value of polyether polyol a was 280.5 mgKOH / g, and the number average molecular weight was 400 Daltons.

[0027] 2. Preparation of polyether polyol b

[0028] The preparation of polyether polyol b comprises the following steps:

[0029] (1) 343 g of m-methoxymethylaniline (Shenzhen Ruijit Biotechnology Co., Ltd.) was added to a 1 L polymerization reactor at room temperature. After nitrogen replacement, the vacuum was turned off. At this time, the pressure in the reactor was -0.1 MPa; the temperature was raised to 110°C.

[0030] (2) First, a mixture of 5 g of ethylene oxide and 45 g of butylene oxide was introduced to raise the pressure in the kettle to 0.35 MPa for induction reaction. When the pressure in the kettle slowly decreased and the temperature gradually increased, it indicated that the induction reaction was successful, and a mixture of 60.7 g of ethylene oxide and 546.3 g of butylene oxide was continuously introduced. During the continuous introduction of the mixture of ethylene oxide and butylene oxide, the pressure in the kettle was controlled to be 0.2 MPa and the temperature in the kettle was controlled to be 110° C. However, during the continuous introduction of the mixture of ethylene oxide and butylene oxide, the polymerization reaction gradually stopped, indicating that although m-methoxymethylaniline contained an amino group, it could not react efficiently with epoxide, and therefore m-methoxymethylaniline had no self-catalytic function.

[0031] 3. Preparation of polyether polyol c

[0032] Preparation of polyether polyol c comprises the following steps:

[0033] (1) 255 g of dimethylaminopropylamine (Shanghai Wandao Chemical Co., Ltd.) was added to a 1 L polymerization reactor at room temperature. After nitrogen substitution, the vacuum was turned off. At this time, the pressure in the reactor was -0.1 MPa; the temperature was raised to 110°C.

[0034] (2) First, a mixture of 5 g of ethylene oxide and 45 g of butylene oxide was introduced to raise the pressure in the autoclave to 0.35 MPa for induction reaction. When the pressure in the autoclave slowly decreased and the temperature gradually increased, it indicated that the induced reaction was successful. Then, a mixture of 69.5 g of ethylene oxide and 675.5 g of butylene oxide was continuously introduced. During the continuous introduction of the mixture of ethylene oxide and butylene oxide, the pressure in the autoclave was controlled to be 0.2 MPa and the temperature in the autoclave was controlled to be 110°C.

[0035] (3) After continuously introducing a mixture of ethylene oxide and butylene oxide, the reaction was carried out at 110°C. When the pressure in the autoclave dropped to -0.1 MPa, the reaction was terminated, the temperature was lowered to 100°C, and vacuum was applied for 1 hour. Finally, the temperature was lowered to room temperature and the material was discharged to obtain polyether polyol c. The hydroxyl value of polyether polyol c was 277 mgKOH / g, and the number average molecular weight was 405 Daltons.

[0036] Example 2 Synthesis of polyether polyols d, e and f

[0037] 1. Synthesizing polyether polyol d, comprising the following reaction steps:

[0038] (1) 233 g of aniline (Shandong Qixing Chemical Co., Ltd.) was added to a 1 L polymerization reactor at room temperature. After nitrogen replacement, the vacuum was turned off. At this time, the pressure in the reactor was -0.1 MPa; the temperature was raised to 110°C.

[0039] (2) First, 50 g of butylene oxide was introduced to raise the pressure in the autoclave to 0.35 MPa for induction reaction. When the pressure in the autoclave slowly decreased and the temperature gradually increased, it indicated that the induction reaction was successful. Then, 717 g of butylene oxide was continuously introduced. During the continuous introduction of butylene oxide, the pressure in the autoclave was controlled to be 0.2 MPa and the temperature in the autoclave was controlled to be 110°C.

[0040] (3) After continuously introducing butylene oxide, the reaction was carried out at 110°C. When the pressure in the autoclave dropped to -0.1 MPa, the reaction was terminated, the temperature was lowered to 100°C, and vacuum was applied for 1 hour. Finally, the temperature was lowered to room temperature and the material was discharged to obtain polyether polyol d. The hydroxyl value of polyether polyol d was 281.9 mgKOH / g, and the number average molecular weight was 398 Daltons.

[0041] 2. Preparation of polyether polyols

[0042] Preparation of polyether polyol e, comprising the following steps:

[0043] (1) 233 g of aniline (Shandong Qixing Chemical Co., Ltd.) was added to a 1 L polymerization reactor at room temperature. After nitrogen replacement, the vacuum was turned off. At this time, the pressure in the reactor was -0.1 MPa; the temperature was raised to 110°C.

[0044] (2) First, a mixture of 7.5 g of ethylene oxide and 42.5 g of butylene oxide was introduced to raise the pressure in the autoclave to 0.35 MPa for induction reaction. When the pressure in the autoclave slowly decreased and the temperature gradually increased, it indicated that the induction reaction was successful. Then, a mixture of 107.6 g of ethylene oxide and 609.4 g of butylene oxide was continuously introduced. During the continuous introduction of the mixture of ethylene oxide and butylene oxide, the pressure in the autoclave was controlled to be 0.2 MPa and the temperature in the autoclave was controlled to be 110°C.

[0045] (3) After continuously introducing the mixture of ethylene oxide and butylene oxide, react at 110°C. When the pressure in the autoclave drops to -0.1 MPa, the reaction is completed, the temperature is lowered to 100°C, and vacuum is applied for 1 hour. Finally, the temperature is lowered to room temperature and the material is discharged to obtain polyether polyol e. The hydroxyl value of polyether polyol e is 279.1 mgKOH / g, and the number average molecular weight is 402 Daltons.

[0046] 3. Preparation of polyether polyols

[0047] Preparation of polyether polyol f, comprising the steps of:

[0048] (1) 233 g of aniline (Shandong Qixing Chemical Co., Ltd.) was added to a 1 L polymerization reactor at room temperature. After nitrogen replacement, the vacuum was turned off. At this time, the pressure in the reactor was -0.1 MPa; the temperature was raised to 110°C.

[0049] (2) First, a mixture of 10 g of ethylene oxide and 40 g of butylene oxide was introduced to raise the pressure in the autoclave to 0.35 MPa for induction reaction. When the pressure in the autoclave slowly decreased and the temperature gradually increased, it indicated that the induced reaction was successful. Then, a mixture of 143.4 g of ethylene oxide and 573.6 g of butylene oxide was continuously introduced. During the continuous introduction of the mixture of ethylene oxide and butylene oxide, the pressure in the autoclave was controlled to be 0.2 MPa and the temperature in the autoclave was controlled to be 110°C.

[0050] (3) After continuously introducing a mixture of ethylene oxide and butylene oxide, the reaction was carried out at 110°C. When the pressure in the autoclave dropped to -0.1 MPa, the reaction was terminated, the temperature was lowered to 100°C, and vacuum was applied for 1 hour. Finally, the temperature was lowered to room temperature and the material was discharged to obtain polyether polyol f. The hydroxyl value of polyether polyol f was 279.8 mgKOH / g, and the number average molecular weight was 401 Daltons.

[0051] Example 3 Synthesis of polyether polyols g, h and m

[0052] 1. Synthesizing polyether polyol g, comprising the following reaction steps:

[0053] (1) 233 g of aniline (Shandong Qixing Chemical Co., Ltd.) and 2 g of potassium hydroxide (Jinan Jiayang Chemical Co., Ltd.) were added to a 1 L polymerization reactor at room temperature. After nitrogen replacement, the vacuum was turned off. At this time, the pressure in the reactor was -0.1 MPa; the temperature was raised to 110°C.

[0054] (2) A mixture of 76.7 g of ethylene oxide and 690.3 g of butylene oxide was continuously introduced. During the process of continuously introducing the mixture of ethylene oxide and butylene oxide, the pressure in the autoclave was controlled to be 0.2 MPa and the temperature in the autoclave was controlled to be 110°C.

[0055] (3) After continuously introducing a mixture of ethylene oxide and butylene oxide, the reaction was carried out at 110°C. When the pressure in the autoclave dropped to -0.1 MPa, the reaction was terminated, the temperature was lowered to 100°C, and vacuum was applied for 1 hour. Finally, the temperature was lowered to room temperature and the material was discharged to obtain polyether polyol g. The hydroxyl value of polyether polyol g was 285.5 mgKOH / g, and the number average molecular weight was 393 Daltons.

[0056] 2. Preparation of polyether polyols

[0057] The preparation of polyether polyol h comprises the following steps:

[0058] (1) 233 g of aniline (Shandong Qixing Chemical Co., Ltd.) and 0.1 g of double metal cyanide complex DMC (Huaian Bader Polyurethane Technology Co., Ltd.) were added to a 1 L polymerization reactor at room temperature. After nitrogen replacement, the vacuum was turned off. At this time, the pressure in the reactor was -0.1 MPa; the temperature was raised to 110°C.

[0059] (2) A mixture of 5 g ethylene oxide and 45 g butylene oxide was first introduced, but the reaction was not successfully induced. The temperature in the autoclave was kept at 140°C for 6 hours after the introduction, and the pressure in the autoclave remained unchanged. This indicates that DMC cannot catalyze the reaction of aniline and epoxide.

[0060] 3. Preparation of polyether polyol m

[0061] Preparation of polyether polyol m, comprising the steps of:

[0062] (1) 233 g of aniline (Shandong Qixing Chemical Co., Ltd.) and 2 g of phosphazene catalyst PZN (Shanghai Qike Fluoro Silicon Material Co., Ltd.) were added into a 1 L polymerization reactor at room temperature. After nitrogen replacement, the vacuum was turned off. At this time, the pressure in the reactor was -0.1 MPa; the temperature was raised to 110°C.

[0063] (2) A mixture of 76.7 g of ethylene oxide and 690.3 g of butylene oxide was continuously introduced. During the process of continuously introducing the mixture of ethylene oxide and butylene oxide, the pressure in the autoclave was controlled to be 0.2 MPa and the temperature in the autoclave was controlled to be 110°C.

[0064] (3) After continuously introducing a mixture of ethylene oxide and butylene oxide, the reaction was carried out at 110°C. When the pressure in the autoclave dropped to -0.1 MPa, the reaction was terminated, the temperature was lowered to 100°C, and vacuum was applied for 1 hour. Finally, the temperature was lowered to room temperature and the material was discharged to obtain polyether polyol m. The hydroxyl value of polyether polyol m was 284.8 mgKOH / g, and the number average molecular weight was 394 Daltons.

[0065] Example 4 Preparation of Adhesive

[0066] Adhesives were prepared using the polyether polyols prepared in Examples 1-3, respectively, and the properties of each adhesive were tested.

[0067] 1. Raw materials of adhesive

[0068] The raw materials of the adhesive include: 100 parts by weight of polyether polyol (a, c, d, e, f, g or m), 80 parts by weight of polymethylene polyphenyl isocyanate, 5 parts by weight of crosslinking agent (ethylene glycol), 0.5 parts by weight of catalyst (dibutyltin dilaurate) and 1.5 parts by weight of thixotropic agent (fumed silica). Among them, polymethylene polyphenyl isocyanate is a mixture of toluene diisocyanate (TDI) and diphenylmethane diisocyanate (MDI) in a mass ratio of 1:1.

[0069] 2. Preparation method of adhesive

[0070] First, the polyether polyol (a, c, d, e, f, g or m) was vacuum dehydrated at 110°C for 2.0h. Polymethylene polyphenyl isocyanate was added to a three-necked flask, and the temperature was raised to 46°C. Then, the dehydrated polyether polyol was added dropwise to the three-necked flask using a dropping funnel. After the addition was completed, the reaction was continued for 0.5 hours, and then the crosslinking agent was added dropwise to continue the reaction for 1h. The temperature was controlled at 46°C during the process of adding the polyether polyol and the crosslinking agent and the reaction. Finally, the temperature was raised to 50°C, the catalyst and thixotropic agent were added, stirred evenly, reacted at 50°C for 30min, and the temperature was lowered to 40°C to obtain the adhesive (A, C, D, E, F, G, M). The polyether polyols in the raw materials of each adhesive are shown in Table 1.

[0071] 3. Adhesive performance test and results

[0072] (1) Performance testing

[0073] The tensile shear strength is tested according to GB / T7124--2008 "Determination of tensile shear strength of adhesives (rigid material to rigid material)". The 180° peel performance is evaluated by the 180° peel strength test of the adhesive specimen composed of two bonded materials, flexible and rigid, under specified conditions, according to GB / T2790--1995 "Adhesive 180° Peel Strength Test Method Flexible Material to Rigid Material". The tensile strength is the load when the tensile force acts on the longitudinal axis of the specimen and is transmitted to the adhesive surface until the specimen is destroyed, for the specimen joint with the bonding surface perpendicular to the longitudinal axis of the specimen, and is tested according to GB / T6329--1996 "Determination of tensile strength of adhesive butt joints". VOC content is tested according to GB / T35609--2017 "Green Product Evaluation Waterproof and Sealing Materials". Water vapor permeability is tested according to GB / T15331--2020 "Test method for water vapor transmission rate of pressure-sensitive adhesive tapes".

[0074] (3) Test results

[0075] The performance test results are shown in Table 1.

[0076] Table 1 Performance test results of adhesives prepared with different polyether polyols

[0077]

[0078] As can be seen from Table 1, the tensile shear strength, 180° peel strength, tensile strength and water vapor permeability of the adhesive A prepared using the polyether polyol a (prepared in Example 1) are significantly higher than those of the adhesives prepared using other polyether polyols. Therefore, the adhesive has high strength, good mechanical properties and environmental protection performance. Since no catalyst is required in the preparation process, the production process is simple, the cost is low, and there is no VOC.

Claims

1. A method for preparing polyether polyol for adhesive, Features The steps include: (1) Adding an amine compound into a polymerization reaction kettle, replacing the atmosphere with nitrogen, and heating the reactor to 90-130° C. and keeping the temperature constant; (2) introducing epoxide and reacting at 90° C. to 120° C.; (3) When the pressure in the autoclave is reduced to negative pressure, the temperature is lowered to 90-110° C., vacuumized, and then lowered to room temperature to obtain the polyether polyol for the adhesive.

2. The preparation method according to claim 1, Features The amine compound is aniline.

3. The preparation method according to claim 1 or 2, Features The epoxide is a mixture of ethylene oxide and butylene oxide.

4. The preparation method according to claim 3, Features The molar ratio of the epoxide to the amine compound is 1-2.5:

1.

5. The preparation method according to claim 4, Features The mass of ethylene oxide in the epoxide accounts for 1% to 50% of the total mass of ethylene oxide and butylene oxide; in the preferred technical scheme, the mass of ethylene oxide in the epoxide accounts for 9% to 12% of the total mass of ethylene oxide and butylene oxide.

6. The preparation method according to claim 5, Features In step (2), a portion of the epoxide is introduced first to induce the reaction, and then the remaining portion of the epoxide is introduced. The mass ratio of the epoxide introduced twice is 1:13-15.

7. The preparation method according to claim 3, Features The number average molecular weight of the polyether polyol for adhesive is 200-500 Daltons.

8. A method for preparing an adhesive, Features The steps include: (1) vacuum dehydrating the polyether polyol prepared by the method according to any one of claims 1 to 7; (2) heating 70-90 parts by weight of polymethylene polyphenyl isocyanate to 42-48° C., then dripping 90-110 parts by weight of the dehydrated polyether polyol described in step (1), reacting at 42-48° C. for 0.3-0.7 hours, dripping 4-6 parts by weight of a crosslinking agent, and continuing to react at 42-48° C. for 0.8-1.2 hours; (3) raising the temperature to 48-52° C., adding 0.4-0.6 parts by weight of a catalyst and 1.3-1.7 parts by weight of a thixotropic agent, reacting for 20-40 minutes, and cooling to room temperature to obtain the adhesive.

9. The preparation method according to claim 8, Features The cross-linking agent is ethylene glycol, the catalyst is dibutyltin dilaurate, the thixotropic agent is fumed silica, and the polymethylene polyphenyl isocyanate is a mixture of toluene diisocyanate and diphenylmethane diisocyanate in a mass ratio of 1:1.