Long-service-life high-resilience high-speed rail bathroom pipe

By using special rubber and PA cord cloth reinforcement layer in high-speed rail bathroom pipes and combining vulcanization treatment, the problems of durability and installation complexity of existing high-speed rail bathrooms are solved, and high-resilience and long-life high-speed rail bathrooms are achieved The tube has good heat resistance and acid and alkali solution resistance, simplifies the installation process and provides shock and noise reduction effect.

CN118909320APending Publication Date: 2024-11-08NANJING ORIENTLEADER TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410964868.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing high-speed rail bathroom pipes are mostly made of stainless steel and plastic. They are complex in installation, short service life, poor elasticity, and are not sufficient to cope with harsh conditions in the use environment.

Method used

The rubber consisting of natural rubber, butyl rubber, zinc oxide, stearic acid, etc. is used as the inner, middle and outer rubber layers, combined with the PA pen fabric reinforcement layer, and the heat resistance and elasticity of the rubber are improved through vulcanization treatment and Acid and alkali-resistant solution performance, and high-resilience high-speed rail bathroom pipes are manufactured through specific structural design and process flow.

Benefits of technology

It realizes the heat resistance, high-temperature pressure degeneration and good rebound of high-speed rail bathroom pipes, simplifies the installation process, extends the service life, and provides shock and noise reduction effects when used.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118909320A_ABST
    Figure CN118909320A_ABST
Patent Text Reader

Abstract

The long-life and high-resilience high-speed rail bathroom pipe sequentially comprises an inner rubber layer, a middle rubber layer and an outer rubber layer from inside to outside, reinforcing layers are arranged at the two ends of the middle rubber layer respectively, each reinforcing layer sequentially comprises a first reinforcing layer and a second reinforcing layer from inside to outside, the outer end of each first reinforcing layer is flush with the outer end of the corresponding second reinforcing layer, and the outer end of each first reinforcing layer is flush with the outer end of the corresponding second reinforcing layer. The first reinforcing layer is shorter than the second reinforcing layer, so that the inner end of the reinforcing layer is step-shaped; the reinforcing layer is made of gum dipping cord fabric formed by gum dipping and calendering of PA cord fabric. The high-speed rail bathroom pipe is light in weight, and the pure glue layer with the reinforcing layers at the two ends and the non-reinforcing layer in the middle is adopted, so that the product is resistant to bending and easier to rebound; the lengths of the two reinforcing layers are different, the outer ends of the first reinforcing layer and the second reinforcing layer are flush, and the length of the first reinforcing layer is smaller than that of the second reinforcing layer, so that the bathroom pipe product is easier to bend, the problem of poor product resilience caused by internal stress concentration is reduced, and the service life is longer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a high-resilience high-speed railway sanitary pipe with long service life. Background Art

[0002] With the rapid development of high-speed rail technology, the demand for bathroom pipes installed in high-speed rail bathrooms is increasing, requiring more attention to intelligence, simplicity, environmental protection and humanization, so as to bring passengers a more comfortable riding experience. In the past, bathroom pipes were mostly made of stainless steel, plastic, etc. The installation of bathroom pipes was relatively complicated, requiring the addition of additional fixings, and the elasticity of bathroom pipes was relatively poor and the service life was short.

[0003] The working principle of the bathroom pipe is as follows: the two ends of the product are fixed with a pinch valve, a certain amount of air pressure is filled from the top, the middle part is completely pressed closed to a non-working state, and the air is pumped to a working state, and the opening and closing cycle is repeated. When the bathroom pipe is working, the middle part will have repeated cycles of complete closure and rebound actions, and good resilience needs to be ensured. In addition, the operating environment of the bathroom pipe is -55℃~+80℃; since feces, weak acid, and weak alkali solutions are generally passed inside the bathroom pipe, it is also necessary to ensure that the bathroom pipe has a certain degree of corrosion resistance. Summary of the invention

[0004] An object of the present invention is to provide a rubber material for preparing an inner rubber layer of a high-speed railway sanitary pipe, the rubber material having heat resistance, high-temperature compression deformation resistance, good resilience and good resistance to acid and alkali solutions; another object of the present invention is to provide a rubber material for dipping used in preparing an intermediate rubber layer, an outer rubber layer or a reinforcing layer of a high-speed railway sanitary pipe, the rubber material having heat resistance, high-temperature compression deformation resistance and good resilience; another object of the present invention is to provide a long-life high-resilience high-speed railway sanitary pipe.

[0005] The objective of the present invention is achieved through the following technical solutions:

[0006] A rubber material for preparing an inner rubber layer of a high-speed railway sanitary pipe is prepared from the following raw materials in parts by weight: 70 to 100 parts of natural rubber, 0 to 30 parts of butadiene rubber, 5 to 15 parts of zinc oxide, 1 to 3 parts of stearic acid, 1 to 3 parts of antioxidant RD, 1 to 3 parts of antioxidant 4010NA, 1 to 3 parts of microcrystalline wax 9108, 50 to 70 parts of carbon black, 1 to 2 parts of flow aid, 2 to 5 parts of tackifying resin, 2 to 3 parts of vulcanizing agent, and 3 to 4 parts of accelerator; wherein the total amount of the natural rubber and butadiene rubber is 100 parts by weight.

[0007] Preferably, the rubber material of the inner rubber layer is made of the following raw materials in parts by weight: 70 to 100 parts of natural rubber, 0 to 30 parts of butadiene rubber, 6 parts of zinc oxide, 1.5 parts of stearic acid, 2 parts of antioxidant RD, 2 parts of antioxidant 4010NA, 1.5 parts of microcrystalline wax 9108, 50 to 70 parts of carbon black, 1 to 2 parts of flow aid, 2 to 5 parts of tackifying resin, 2.5 parts of vulcanizing agent, and 3.25 to 3.5 parts of accelerator.

[0008] Most preferably, the rubber material of the inner rubber layer is made of the following raw materials in parts by weight: 70 to 100 parts of natural rubber, 0 to 30 parts of butadiene rubber, 6 parts of zinc oxide, 1.5 parts of stearic acid, 2 parts of antioxidant RD, 2 parts of antioxidant 4010NA, 1.5 parts of microcrystalline wax 9108, 50 to 70 parts of carbon black, 1 to 2 parts of flow aid, 2 to 5 parts of tackifying resin, 2.5 parts of vulcanizing agent, and 3.25 parts of accelerator.

[0009] The Mooney viscosity of the natural rubber is 45 to 75 (ML (1+4) 100°C). Specifically, the natural rubber can be selected from SVR CV60.

[0010] The Mooney viscosity of the butadiene rubber is 40 to 100 (ML (1+4) 100°C). Specifically, the butadiene rubber can be selected from butadiene rubber BR 9000.

[0011] The carbon black is carbon black N550.

[0012] The flow aid is STRUKTOL WB222.

[0013] The tackifying resin is coumarone resin.

[0014] The vulcanizing agent is insoluble sulfur IS60-75GE F500.

[0015] The accelerator is a combination of accelerator DTDM-80, accelerator DM (MBTS) and accelerator CZ (CBS) in a weight ratio of (2.5-5):1:(3.5-7), preferably a combination of accelerator DTDM-80, accelerator DM and accelerator CZ in a weight ratio of 5:1:7.

[0016] A method for preparing a rubber material for preparing an inner rubber layer of a high-speed railway sanitary pipe comprises the following steps:

[0017] Step (1), cooling water is passed through the internal mixer, the temperature of the internal mixer working room is controlled at 45-55° C., the rotation speed is 32-35 rpm, raw rubber is added, and internal mixing is performed for 1-2 minutes, and then zinc oxide, stearic acid, antioxidant RD, antioxidant 4010NA, microcrystalline wax 9108, flow aid, and tackifying resin are added, and mixing is performed for 5-6 minutes;

[0018] Step (2), cooling water is continued to flow through the internal mixer, carbon black is added to the internal mixer for mixing, and when the temperature of the internal mixer reaches 95° C., an accelerator and a vulcanizing agent are added, and when the temperature of the internal mixer reaches 105-110° C., rubber discharge is performed by adjusting the roller spacing of the open mixer to 0.1 mm, making 2 triangle packages, adjusting the roller spacing to 0.5 mm, making 2 rolls, adjusting the roller spacing of the open mixer to 3.0 mm, and discharging a sheet to obtain a rubber material for preparing an inner rubber layer.

[0019] A rubber material for preparing an intermediate rubber layer, a dipping layer of a reinforcement layer or an outer rubber layer of a high-speed railway sanitary pipe, which is made of the following raw materials in parts by weight: 100 parts of natural rubber, 5 to 15 parts of zinc oxide, 1 to 3 parts of stearic acid, 1 to 3 parts of antioxidant RD, 1 to 3 parts of antioxidant 4010NA, 1 to 3 parts of microcrystalline wax 9108, 2 to 5 parts of tackifying resin, 1 to 2 parts of flow aid, 5 to 10 parts of plasticizer, 15 to 35 parts of carbon black, 2 to 3 parts of vulcanizing agent, and 3 to 4 parts of accelerator.

[0020] Preferably, the rubber material for the intermediate rubber layer, the impregnation layer of the reinforcement layer or the outer rubber layer for preparing the long-life high-resilience high-speed railway sanitary pipe is made of the following raw materials in parts by weight: 100 parts of natural rubber, 6 parts of zinc oxide, 1.5 parts of stearic acid, 2 parts of antioxidant RD, 2 parts of antioxidant 4010NA, 1.5 parts of microcrystalline wax 9108, 2 to 5 parts of tackifying resin, 1 to 2 parts of flow aid, 5 to 10 parts of plasticizer, 15 to 35 parts of carbon black, 2.5 parts of vulcanizing agent, and 2.75 to 3.75 parts of accelerator.

[0021] Most preferably, the rubber material for the intermediate rubber layer, the impregnation layer of the reinforcement layer or the outer rubber layer for preparing a long-life and high-resilience high-speed railway sanitary pipe is made of the following raw materials in parts by weight: 100 parts of natural rubber, 6 parts of zinc oxide, 1.5 parts of stearic acid, 2 parts of antioxidant RD, 2 parts of antioxidant 4010NA, 1.5 parts of microcrystalline wax 9108, 2 to 5 parts of tackifying resin, 1 to 2 parts of flow aid, 5 to 10 parts of plasticizer, 15 to 35 parts of carbon black, 2.5 parts of vulcanizing agent, and 3.25 parts of accelerator.

[0022] The Mooney viscosity of the natural rubber is 45 to 75 (ML (1+4) 100° C.). Specifically, the natural rubber can be selected from natural rubber SVR CV60.

[0023] The carbon black is carbon black STERLING NS.

[0024] The flow aid is STRUKTOL WB222.

[0025] The tackifying resin is coumarone resin.

[0026] The plasticizer is plasticizer UN488.

[0027] The vulcanizing agent is insoluble sulfur IS60-75GE F500.

[0028] The accelerator is a combination of accelerator DTDM-80, accelerator DM and accelerator CZ in a weight ratio of 5:(2-6):4, preferably a combination of accelerator DTDM-80, accelerator DM and accelerator CZ in a weight ratio of 5:4:4.

[0029] A method for preparing a rubber material for preparing an intermediate rubber layer, a reinforcement layer or an outer rubber layer of a high-speed railway sanitary pipe comprises the following steps:

[0030] Step (1), cooling water is passed through the internal mixer, the temperature of the internal mixer working room is controlled at 45-55° C., the rotation speed is 32-35 rpm, natural rubber is added, and the internal mixer is kneaded for 1-2 minutes, and then zinc oxide, stearic acid, antioxidant RD, antioxidant 4010NA, microcrystalline wax 9108, flow aid, and tackifying resin are added, and the mixture is kneaded for 5-6 minutes;

[0031] Step (2), cooling water is continued to flow through the internal mixer, carbon black and plasticizer are added to the internal mixer for mixing, and when the temperature of the internal mixer reaches 95° C., accelerators and vulcanizers are added, and when the temperature of the internal mixer reaches 105-110° C., rubber removal is performed by adjusting the roller spacing of the open mixer to 0.1 mm, making 2 triangle packages, adjusting the roller spacing to 0.5 mm, making 2 rolls, adjusting the roller spacing of the open mixer to 3.0 mm, and discharging sheets to obtain a rubber material for preparing an intermediate rubber layer, a reinforcing layer, or an outer rubber layer.

[0032] A long-life high-resilience high-speed railway sanitary pipe, the sanitary pipe comprises an inner rubber layer, an intermediate rubber layer and an outer rubber layer from the inside to the outside, reinforcement layers are respectively arranged at both ends of the intermediate rubber layer, the reinforcement layers comprise a first reinforcement layer and a second reinforcement layer from the inside to the outside, the outer ends of the first reinforcement layer and the second reinforcement layer are flush, and the length of the first reinforcement layer is shorter than the length of the second reinforcement layer so that the inner ends of the reinforcement layers are stepped; the rubber material of the inner rubber layer is the rubber material of the inner rubber layer used to prepare the high-speed railway sanitary pipe, the rubber materials of the intermediate rubber layer and the outer rubber layer are the rubber materials of the intermediate rubber layer, the reinforcement layer or the outer rubber layer used to prepare the high-speed railway sanitary pipe; the material of the reinforcement layer is a dipped rubber cord cloth formed by dipping and calendering the rubber material of the intermediate rubber layer, the reinforcement layer or the outer rubber layer used to prepare the high-speed railway sanitary pipe.

[0033] Preferably, the sanitary pipe comprises an inner rubber layer, a middle rubber layer and an outer rubber layer from the inside to the outside, and reinforcement layers are respectively provided at both ends of the middle rubber layer. The reinforcement layers comprise a first reinforcement layer and a second reinforcement layer from the inside to the outside, the outer ends of the first reinforcement layer and the second reinforcement layer are flush, and the length of the first reinforcement layer is shorter than the length of the second reinforcement layer so that the inner ends of the reinforcement layers are stepped; the middle rubber layer is a whole composed of a first middle rubber layer, a second middle rubber layer and a third middle rubber layer from the inside to the outside, the thickness of the middle rubber layer is greater than the thickness of the reinforcement layer, the thickness of the second middle rubber layer is the same as the thickness of the first reinforcement layer, and the thickness of the third middle rubber layer is the same as the thickness of the second reinforcement layer.

[0034] The thickness of the inner rubber layer is 2.0-2.1 mm, the thickness of the middle layer is 1.6-1.7 mm; the thickness of the first reinforcement layer is 0.55-65 mm; the thickness of the second reinforcement layer is 0.55-0.65 mm; the thickness of the outer rubber layer is 3.1-3.2 mm.

[0035] The length of the bathroom pipe is 118-123 mm.

[0036] The dipped cord fabric is formed by dipping and calendering the intermediate rubber layer, the reinforcement layer or the outer rubber layer of the high-speed railway sanitary pipe using about 1 kg of the dipped rubber per square meter of PA cord fabric.

[0037] The PA cord fabric is PA66 cord fabric.

[0038] Another object of the present invention is to provide a method for preparing the long-life high-resilience high-speed railway sanitary pipe, comprising the following steps:

[0039] Step (1), using an extruder to extrude the rubber material of the inner rubber layer onto a mandrel coated with a release agent to obtain an inner rubber layer with a mandrel;

[0040] Step (2), using a winding machine to wrap the rubber material of the middle rubber layer around the inner rubber layer to form a first middle rubber layer;

[0041] Step (3), respectively wrapping the dipped cord fabric at both ends of the intermediate rubber at an angle of 36° to form a first reinforcement layer, corresponding to the first reinforcement layer, using a winding machine to wind a circle of rubber material of the intermediate rubber layer with the same thickness as the first reinforcement layer on the outside of the middle of the intermediate rubber layer, to form a second intermediate rubber layer; cross-wrapping the dipped cord fabric at an angle of 36° on the outside of the first reinforcement layer to form a second reinforcement layer, corresponding to the second reinforcement layer, using a winding machine to wind a circle of rubber material of the intermediate rubber layer with the same thickness as the second reinforcement layer on the outside of the middle of the intermediate rubber layer, to form a third intermediate rubber layer;

[0042] Step (4), using a winding machine to wind the rubber material of the outer rubber layer around the reinforcing layer and the middle rubber layer to form an outer rubber layer, thereby obtaining a tube blank;

[0043] Step (5), taking out the tube blank;

[0044] Step (6), inflating the inner bag, evacuating the vacuum, and vulcanizing in a vulcanizing tank, the vulcanizing temperature is 150-165° C., the vulcanizing pressure is 2.3-2.4 MPa, and the vulcanizing time is 25-60 min to obtain a high-speed railway sanitary pipe.

[0045] Beneficial effects of the present invention:

[0046] In terms of rubber: an effective vulcanization system is used to make the rubber have better compression deformation and heat resistance.

[0047] In terms of structure: the high-speed rail sanitary pipe is light in weight, and adopts a pure rubber layer with reinforcement layers at both ends and no reinforcement layer in the middle, so that the product is resistant to bending and easier to rebound; the lengths of the two reinforcement layers are inconsistent, and the outer ends of the first reinforcement layer and the second reinforcement layer are flush, and the length of the first reinforcement layer is shorter than that of the second reinforcement layer, which makes the sanitary pipe product easier to bend, reduces the problem of poor product rebound caused by internal stress concentration, and has a longer service life.

[0048] The high-speed railway bathroom pipe of the present invention is thicker, has a cord fabric inside and has good elasticity, and can play a role in shock absorption and noise reduction when in use; when installing, it only needs to be clamped with an air clamp valve, and the installation is relatively simple and more convenient. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 This is a schematic diagram of the structure of the high-speed railway bathroom pipe of the present invention;

[0050] Figure 2 This is a partial enlarged view of the high-speed railway bathroom pipes.

[0051] In the figure, 1-inner rubber layer, 2-middle rubber layer, 3-first reinforcement layer, 4-second reinforcement layer, 5-outer rubber layer.

[0052] Figure 3 This is a real picture of the high-speed railway bathroom pipe in Example 7 when it is folded and clamped (A) and after it rebounds (B). DETAILED DESCRIPTION

[0053] The technical solution of the present invention is further described below through specific implementation methods.

[0054] Table 1. Formula of inner layer rubber (parts by weight)

[0055]

[0056] Example 1

[0057] The raw materials and weight proportions of the rubber material used to prepare the inner rubber layer of the high-speed railway sanitary pipe are shown in Table 1. It is prepared by the following method, and the steps are as follows:

[0058] Step (1), cooling water is passed through the internal mixer, the temperature of the internal mixer working room is controlled at 55° C., the rotation speed is 32 rpm, raw rubber (natural rubber SVR CV60) is added, and the internal mixing is performed for 2 minutes, and then zinc oxide, stearic acid, antioxidant RD, antioxidant 4010NA, microcrystalline wax 9108, flow aid STRUKTOL WB222, and coumarone resin are added, and the mixture is mixed for 3 minutes;

[0059] Step (2), cooling water is continued to flow through the internal mixer, carbon black is added to the internal mixer for mixing, and when the temperature of the internal mixer reaches 95° C., accelerator DTDM-80, accelerator DM, accelerator CZ, and vulcanizing agent IS60-75GE F500 are added, and when the temperature of the internal mixer reaches 108° C., rubber removal is performed by adjusting the roller spacing of the open mixer to 0.1 mm, making 2 triangle packages, adjusting the roller spacing to 0.5 mm, making 2 rolls, adjusting the roller spacing of the open mixer to 3.0 mm, discharging the sheet, and cooling to room temperature at room temperature to obtain a rubber material for the inner rubber layer.

[0060] Example 2

[0061] On the basis of Example 1, the amount of natural rubber SVR CV60 was adjusted to 85 parts and the amount of butadiene rubber BR 9000 was adjusted to 15 parts. The specific formula is shown in Table 1. The raw materials were weighed according to Table 1, and the rubber material for the inner rubber layer was prepared by referring to the preparation method of Example 1.

[0062] Example 3

[0063] On the basis of Example 1, the amount of natural rubber SVR CV60 was adjusted to 70 parts and the amount of butadiene rubber BR 9000 was adjusted to 30 parts. The specific formula is shown in Table 1. The raw materials were weighed according to Table 1, and the rubber material for the inner rubber layer was prepared by referring to the preparation method of Example 1.

[0064] Example 4

[0065] On the basis of Example 1, the amount of natural rubber SVR CV60 was adjusted to 70 parts, the amount of butadiene rubber BR 9000 was adjusted to 30 parts, and the amount of accelerator DM was adjusted to 0.5 parts. The specific formula is shown in Table 1. The raw materials were weighed according to Table 1, and the rubber material for the inner rubber layer was prepared by referring to the preparation method of Example 1.

[0066] Comparative Example 1

[0067] On the basis of Example 1, the dosage of the accelerator DM was adjusted to 0, the raw materials were weighed according to Table 1, and the rubber material was prepared by referring to the preparation method of Example 1.

[0068] Comparative Example 2

[0069] On the basis of Example 2, the dosage of the accelerator DM was adjusted to 0, the raw materials were weighed according to Table 1, and the rubber material was prepared by referring to the preparation method of Example 1.

[0070] Comparative Example 3

[0071] On the basis of Example 3, the dosage of the accelerator DM was adjusted to 0, the raw materials were weighed according to Table 1, and the rubber material was prepared by referring to the preparation method of Example 1.

[0072] Take the required rubber materials and vulcanize them separately. The steps are as follows:

[0073] Step (1), setting the vulcanization parameters of the flat vulcanizing press: temperature 150°C, pressure 15MPa, time 1200s;

[0074] Step (2), when the vulcanizing temperature of the flat plate vulcanizer reaches 150°C, place the test piece and the compression block sample;

[0075] Step (3), ensuring that the vulcanization temperature is 150° C., after the vulcanization time is reached, opening the mold and sampling to obtain the vulcanized rubber.

[0076] The properties of the rubber material (vulcanized rubber) of the inner rubber layer were tested, see Table 2.

[0077] Table 2. Performance parameters of the rubber compound of the inner rubber layer

[0078]

[0079] Note: pH value of acid solution: 0.80; pH value of alkaline solution: 13.66.

[0080] It can be seen from Table 2 that with the increase of the amount of butadiene rubber BR 9000, the conventional Shore A hardness, tensile strength and elongation at break slightly decreased, the change of heat aging hardness and tensile strength change rate slightly improved, the change rate of elongation at break did not change much, the rebound performance improved greatly, the high temperature compression performance slightly improved, the low temperature brittleness improved significantly, and the acid and alkali solution resistance improved; compared with the corresponding comparative example, the accelerator DM was added to Examples 1-3, the conventional Shore A hardness and tensile strength were improved, and the elongation at break slightly decreased, indicating that the crosslinking degree of the rubber was improved, and the heat aging performance, high temperature compression performance and acid and alkali solution resistance performance were further improved, indicating that the accelerator DM can improve the crosslinking degree of the rubber and improve the heat resistance and compression performance; compared with Example 3, Example 4 increased the amount of accelerator DM, and the heat aging and compression performance decreased slightly, but it was still better than the rubber without adding accelerator DM. The rubber obtained in Example 3 has the best comprehensive performance, especially the compression performance is better.

[0081] Table 3. Formulation of the rubber material of the middle rubber layer (reinforcement layer dipping, outer rubber layer) (parts by weight)

[0082]

[0083] Example 5

[0084] The rubber material used to prepare the intermediate rubber layer, the impregnation of the reinforcement layer or the outer rubber layer of the high-speed railway sanitary pipe is the same. The raw materials and weight proportions of the rubber material are shown in Table 3. The rubber material is prepared by the following method, and the steps are as follows:

[0085] Step (1), cooling water is passed through the internal mixer, the temperature of the internal mixer working room is controlled at 55° C., the speed is 32 rpm, natural rubber SVR CV60 is added, and the internal mixing is performed for 2 minutes, and then zinc oxide, stearic acid, antioxidant RD, antioxidant 4010NA, microcrystalline wax 9108, flow aid STRUKTOL WB222, and coumarone resin are added and mixed for 3 minutes;

[0086] Step (2), cooling water is continued to flow through the internal mixer, carbon black STERLING NS and plasticizer UN488 are added to the internal mixer for mixing, and when the temperature of the internal mixer reaches 95° C., accelerator DTDM-80, accelerator DM, accelerator CZ, and vulcanizer IS60-75GEF500 are added, and when the temperature of the internal mixer reaches 108° C., rubber discharge is carried out by adjusting the roller spacing of the open mixer to 0.1 mm, making 2 triangle bags, adjusting the roller spacing to 0.5 mm, making 2 rolls, adjusting the roller spacing of the open mixer to 3.0 mm, discharging sheets, and cooling to room temperature at room temperature to obtain a rubber material.

[0087] Example 6

[0088] On the basis of Example 5, the dosage of the accelerator DM was adjusted to 1 part. The specific formula is shown in Table 3. The raw materials were weighed according to Table 3, and the rubber material was prepared by referring to the preparation method of Example 5.

[0089] Example 7

[0090] On the basis of Example 5, the dosage of the accelerator DM was adjusted to 1.5 parts. The specific formula is shown in Table 3. The raw materials were weighed according to Table 3, and the rubber material was prepared by referring to the preparation method of Example 5.

[0091] Comparative Example 4

[0092] On the basis of Example 5, the dosage of the accelerator DM was adjusted to 0. The specific formula is shown in Table 3. The raw materials were weighed according to Table 3, and the rubber material was prepared by referring to the preparation method of Example 5.

[0093] Take the required rubber materials and vulcanize them separately. The steps are as follows:

[0094] Step (1), setting the vulcanization parameters of the flat vulcanizing press: temperature 150°C, pressure 15MPa, time 1200s;

[0095] Step (2), when the vulcanizing temperature of the flat plate vulcanizer reaches 150°C, place the test piece and the compression block sample;

[0096] Step (3), ensuring that the vulcanization temperature is 150° C., after the vulcanization time is reached, opening the mold and sampling to obtain the vulcanized rubber.

[0097] The properties of the intermediate rubber layer, the impregnation of the reinforcement layer or the rubber (vulcanized rubber) of the outer rubber layer are tested, see Table 4.

[0098] Table 4. Performance parameters of the rubber materials for the intermediate rubber layer, the reinforcement layer or the outer rubber layer

[0099]

[0100] It can be seen from Table 4 that as the amount of accelerator DM increases, the conventional hardness of the rubber increases, the tensile strength and elongation at break decrease, and the heat aging performance, resilience, and high temperature compression are significantly improved. The rubber obtained in Example 6 has the best comprehensive performance, especially the compression performance.

[0101] Example 8

[0102] like Figure 1 and Figure 2 As shown, a long-life high-resilience high-speed railway sanitary pipe, the inner diameter of the sanitary pipe is 48mm, the hose comprises an inner rubber layer 1, an intermediate rubber layer 2, an outer rubber layer 5 from the inside to the outside, and reinforcement layers are respectively arranged at both ends of the intermediate rubber layer 2, the reinforcement layers are sequentially a first reinforcement layer 3 and a second reinforcement layer 4 from the inside to the outside, the outer ends of the first reinforcement layer 3 and the second reinforcement layer 4 are flush, and the length of the first reinforcement layer 3 is shorter than the length of the second reinforcement layer 4 so that the inner end of the reinforcement layer is stepped; the intermediate rubber layer 2 is sequentially a first intermediate rubber layer, a second intermediate rubber layer 4 from the inside to the outside and the third intermediate rubber layer, the thickness of the intermediate rubber layer is greater than the thickness of the reinforcement layer, the thickness of the second intermediate rubber layer is the same as the thickness of the first reinforcement layer 3, and the thickness of the third intermediate rubber layer is the same as the thickness of the second reinforcement layer 4; the rubber material of the inner rubber layer 1 is the rubber material prepared in Example 3, and the rubber materials of the intermediate rubber layer 2 and the outer rubber layer 5 are both the rubber material prepared in Example 6; the materials of the first reinforcement layer and the second reinforcement layer are both dipped tire cord fabrics formed by dipping and calendering about 1 kg of the rubber material prepared in Example 6 per square meter of PA66 tire cord fabric.

[0103] The thickness of the inner rubber layer 1 is 2.0 mm and the length is 120 mm; the thickness of the middle rubber layer 2 is 1.6 mm and the length is 120 mm; the total thickness of the reinforcement layer is 1.2 mm; the thickness of the outer rubber layer is 3.2 mm and the length is 120 mm.

[0104] The first reinforcement layer 3 has a thickness of 0.6 mm and a width of 29 mm, the second intermediate rubber layer has a thickness of 0.6 mm and a width of 62 mm; the second reinforcement layer 4 has a thickness of 0.6 mm and a width of 39 mm, the third intermediate rubber layer has a thickness of 0.6 mm and a width of 42 mm; the length of the bathroom pipe is 120 mm.

[0105] The high-speed railway sanitary ware pipe of this embodiment is prepared by the following preparation method, which includes the following steps:

[0106] Step (1), applying a release agent GC-4800B on the core rod; using an extruder to extrude the rubber material prepared in Example 3 onto the core rod coated with the release agent to obtain an inner rubber layer with a core shaft;

[0107] Step (2), using a winding machine to wrap the rubber material of the middle rubber layer prepared in Example 6 around the inner rubber layer, and removing excess rubber material at the overlapping part, to form a first middle rubber layer;

[0108] Step (3), respectively wrapping the dipped cord fabric at both ends of the intermediate rubber at an angle of 36° to form a first reinforcement layer, corresponding to the first reinforcement layer, using a winding machine to wind a circle of intermediate rubber with the same thickness as the first reinforcement layer on the outside of the middle of the intermediate rubber layer, removing excess rubber from the overlapping part, and forming a second intermediate rubber layer; wrapping the dipped cord fabric at an angle of 36° to form a second reinforcement layer on the outside of the first reinforcement layer, corresponding to the second reinforcement layer, using a winding machine to wind a circle of intermediate rubber with the same thickness as the second reinforcement layer on the outside of the middle of the intermediate rubber layer, removing excess rubber from the overlapping part, and forming a third intermediate rubber layer;

[0109] Step (4), using a winding machine to wind the rubber material of the outer rubber layer prepared in Example 6 around the reinforcing layer and the intermediate rubber layer to form an outer rubber layer, and removing excess rubber material from the overlapping part to obtain a tube blank;

[0110] Step (6), using an air gun to properly inflate and remove the tube blank;

[0111] Step (7), inflating the inner bag, evacuating the air, and vulcanizing in a vulcanizing tank, the vulcanizing temperature is 150° C., the vulcanizing pressure is 2.3 MPa, and the vulcanizing time is 50 min, to obtain a high-speed railway sanitary pipe.

[0112] Fold the high-speed railway bathroom pipe of this embodiment in half and clamp it ( Figure 3 A), placed at room temperature for 7 days, the compression-rebound effect is good, and then folded and clamped and placed at 80℃ for 3 days, the compression-rebound effect is good ( Figure 3 B).

Claims

1. A rubber material for preparing the inner rubber layer of a high-speed railway sanitary pipe, characterized in that: It is made of the following raw materials in parts by weight: 70 to 100 parts of natural rubber, 0 to 30 parts of butadiene rubber, 5 to 15 parts of zinc oxide, 1 to 3 parts of stearic acid, 1 to 3 parts of antioxidant RD, 1 to 3 parts of antioxidant 4010NA, 1 to 3 parts of microcrystalline wax 9108, 50 to 70 parts of carbon black, 1 to 2 parts of flow aid, 2 to 5 parts of tackifying resin, 2 to 3 parts of vulcanizing agent, and 3 to 4 parts of accelerator; wherein the total amount of the natural rubber and butadiene rubber is 100 parts by weight.

2. The rubber material for preparing the inner rubber layer of the high-speed railway sanitary pipe according to claim 1, characterized in that: It is made of the following raw materials in parts by weight: 70-100 parts of natural rubber, 0-30 parts of butadiene rubber, 6 parts of zinc oxide, 1.5 parts of stearic acid, 2 parts of antioxidant RD, 2 parts of antioxidant 4010NA, 1.5 parts of microcrystalline wax 9108, 50-70 parts of carbon black, 1-2 parts of flow aid, 2-5 parts of tackifying resin, 2.5 parts of vulcanizing agent, and 3.25-3.5 parts of accelerator.

3. The rubber material for preparing the inner rubber layer of the high-speed railway sanitary pipe according to claim 1 or 2, characterized in that: The Mooney viscosity of the natural rubber is 45 to 75 (ML (1+4) 100°C); the Mooney viscosity of the butadiene rubber is 40 to 100 (ML (1+4) 100℃).

4. The rubber material for preparing the inner rubber layer of the high-speed railway sanitary pipe according to claim 1 or 2, characterized in that: The carbon black is carbon black N550; the flow aid is STRUKTOL WB222; the tackifying resin is coumarone resin; the vulcanizing agent is insoluble sulfur IS60-75GE F500; the accelerator is a combination of accelerator DTDM-80, accelerator DM and accelerator CZ in a weight ratio of (2.5-5):1:(3.5-7), preferably a combination of accelerator DTDM-80, accelerator DM and accelerator CZ in a weight ratio of 5:1:

7.

5. A rubber material for preparing an intermediate rubber layer, a reinforcement layer or an outer rubber layer of a high-speed railway sanitary pipe, characterized in that: The invention is prepared from the following raw materials in parts by weight: 100 parts of natural rubber, 5 to 15 parts of zinc oxide, 1 to 3 parts of stearic acid, 1 to 3 parts of antioxidant RD, 1 to 3 parts of antioxidant 4010NA, 1 to 3 parts of microcrystalline wax 9108, 2 to 5 parts of tackifying resin, 1 to 2 parts of flow aid, 5 to 10 parts of plasticizer, 15 to 35 parts of carbon black, 2 to 3 parts of vulcanizing agent and 3 to 4 parts of accelerator.

6. The rubber material for preparing the intermediate rubber layer, the impregnation of the reinforcement layer or the outer rubber layer of the high-speed railway sanitary pipe according to claim 5, characterized in that: The invention is prepared from the following raw materials in parts by weight: 100 parts of natural rubber, 6 parts of zinc oxide, 1.5 parts of stearic acid, 2 parts of antioxidant RD, 2 parts of antioxidant 4010NA, 1.5 parts of microcrystalline wax 9108, 2-5 parts of tackifying resin, 1-2 parts of flow aid, 5-10 parts of plasticizer, 15-35 parts of carbon black, 2.5 parts of vulcanizing agent and 2.75-3.75 parts of accelerator.

7. The rubber material for preparing the intermediate rubber layer, the impregnation of the reinforcement layer or the outer rubber layer of the high-speed railway sanitary pipe according to claim 5 or 6, characterized in that: The Mooney viscosity of the natural rubber is 45 to 75 (ML (1+4) 100℃).

8. The rubber material for preparing the intermediate rubber layer, the impregnation of the reinforcement layer or the outer rubber layer of the high-speed railway sanitary pipe according to claim 5 or 6, characterized in that: The carbon black is carbon black STERLING NS; the flow aid is STRUKTOL WB222; the tackifying resin is coumarone resin; the plasticizer is plasticizer UN488; the vulcanizing agent is insoluble sulfur IS60-75GE F500; the accelerator is a combination of accelerator DTDM-80, accelerator DM and accelerator CZ in a weight ratio of 5:(2-6):4, preferably a combination of accelerator DTDM-80, accelerator DM and accelerator CZ in a weight ratio of 5:4:

4.

9. A long-life high-rebound high-speed railway bathroom pipe, characterized by: The bathroom pipe comprises an inner rubber layer, an intermediate rubber layer, and an outer rubber layer from the inside to the outside, and reinforcement layers are respectively provided at both ends of the intermediate rubber layer. The reinforcement layers comprise a first reinforcement layer and a second reinforcement layer from the inside to the outside, and the outer ends of the first reinforcement layer and the second reinforcement layer are flush, and the length of the first reinforcement layer is shorter than the length of the second reinforcement layer so that the inner end of the reinforcement layer is stepped; the rubber material of the inner rubber layer is the rubber material described in claim 1, and the rubber materials of the intermediate rubber layer and the outer rubber layer are both the rubber material described in claim 5; the material of the reinforcement layer is a dipped cord fabric made by dipping and calendering PA cord fabric using the rubber material described in claim 5.

10. The long-life high-resilience high-speed railway sanitary pipe according to claim 9, characterized in that: The intermediate rubber layer is a whole composed of the first intermediate rubber layer, the second intermediate rubber layer and the third intermediate rubber layer from the inside to the outside. The thickness of the intermediate rubber layer is greater than the thickness of the reinforcement layer, and the thickness of the second intermediate rubber layer is the same as the thickness of the first reinforcement layer, and the thickness of the third intermediate rubber layer is the same as the thickness of the second reinforcement layer.

Citation Information

Cited By

  • Heat-resistant long-life high-resilience clip tube valve rubber tube