UHMWPE / HDPE composite material and preparation method thereof

The high-oriented microfibrosis of UHMWPE in HDPE matrix is ​​achieved through micro-nano stacking and co-extrusion technology, which solves the problems of processing difficulties and mechanical properties of UHMWPE materials, improves the strength and crystallization performance of composite materials, simplifies the preparation process and improves the preparation process. Productivity.

CN118909338APending Publication Date: 2024-11-08QUANGANG PETROCHEM RES INST OF FUJIAN NORMAL UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410974709.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The ultra-long molecular chains and high molecular weight of existing UHMWPE materials lead to large melt viscosity and difficult processing and forming. The application in polyolefin matrix has chain entanglement problems, which affects its mechanical properties.

Method used

Using micro-nano stacking co-extrusion technology, the distribution and arrangement orientation of UHMWPE in the HDPE matrix is ​​realized through the strong shear and tensile flow field in the stacker, forming high-oriented microfibers along the longitudinal direction, reducing molecular chain entanglement. to improve material strength.

Benefits of technology

Effectively solves the problems of processing and forming difficulties and mechanical properties of UHMWPE materials, improves the strength and crystallization properties of composite materials, realizes uniform dispersion and oriented fiber formation in HDPE matrix, simplifies the preparation method, improves production efficiency and industrialization ability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004954199750000051
    Figure BDA0004954199750000051
Patent Text Reader

Abstract

The invention discloses a UHMWPE (ultrahigh molecular weight polyethylene) / HDPE (high-density polyethylene) composite material and a preparation method thereof. The UHMWPE / HDPE composite material is prepared from 100 parts by weight of HDPE and 10-50 parts by weight of UHMWPE through micro-nano lamination extrusion equipment, a multi-layer PE micro-layer structure which is arranged in parallel in the sheet extension direction is formed, and UHMWPE fibers are arranged in order in the extrusion direction. Strong shear and tensile force fields in the laminator can improve the crystallization property and microstructure of the PE material and enhance the orientation of a PE molecular chain in the flowing direction, meanwhile, the melting point of the UHMWPE is slightly higher than that of HDPE, and the UHMWPE which is not completely molten forms fibers in an interlayer interface under the action of the strong shear and tensile force fields, so that the mechanical strength of the composite material is further improved. According to the method, uniform dispersion and oriented fiber forming of UHMWPE in an HDPE base material are achieved through the micro-nano lamination technology, the strength of the composite material is improved, the preparation method is simple, the production efficiency is high, and continuous batch production can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer material processing, and in particular relates to a UHMWPE / HDPE composite material and a preparation method thereof. Background Art

[0002] Polyethylene (PE) is a thermoplastic synthesized by polymerizing ethylene (CH2=CH2) monomers. As the simplest polymer material, it has good mechanical properties, corrosion resistance, friction resistance, low price and easy processing, and is widely used in the manufacture of pipes, films, containers, fibers, wires, cables, household appliances and daily necessities. According to its properties, polyethylene can be divided into several types, such as LDPE (low-density polyethylene), LLDPE (linear low-density polyethylene) and HDPE (high-density polyethylene). Among them, each molecule of HDPE has 700 to 1800 monomer units, a molecular weight of tens of thousands to hundreds of thousands, and has the characteristics of low branch content, high crystallinity, and high melting point. It has high strength, toughness and creep resistance, and is widely used in extrusion blow molding containers, pipes, wires and cables, and packaging materials. Ultra-high molecular weight polyethylene (UHMWPE) has more than 100,000 monomer units per molecule, and a molecular weight of millions, usually between 2 and 6 million. As one of the high-end polyethylene materials, UHMWPE has good impact resistance, corrosion resistance, friction resistance and self-lubrication. At present, in the existing UHMWPE commercial resin, due to its ultra-long molecular chain and ultra-high molecular weight, there are a large number of physical entanglement points between and within the molecular chains, which restricts the creep and relaxation behavior of long-chain polyethylene, resulting in extremely high melt viscosity of UHMWPE, crystal defects, and difficulties in material processing and molding. Therefore, reducing the chain entanglement degree of UHMWPE can not only improve its own processing performance, but also increase its blendable amount in polyolefins, and obtain high-performance polyethylene materials with greatly enhanced mechanical properties.

[0003] In order to solve the above problems, the preparation process of ultra-high molecular weight polyethylene / polyolefin blends by nanoscale blending has become a research hotspot. This method has the advantages of good compatibility of each component, excellent processing performance, environmental friendliness and recyclability. Micro-nano lamination technology, also known as multi-layer co-extrusion technology, is a new type of melt processing technology. It connects multiple laminators in series after traditional extrusion operation, and can be used to synthesize multi-layer polymer composites ranging from nanometer to micrometer scale in a molten state. The polymer melt undergoes splitting, diffusion and stacking in the laminator. In this process, not only the flow channel of the melt is extended, but also the polymer melt is subjected to continuous shear force and tensile force. These force fields help to improve the distribution and morphological adjustment of the dispersed phase in the matrix. By utilizing the convergent stretching effect in the laminator, the chain entanglement degree of UHMWPE can be reduced, and it can be elongated to form micro-nanoscale fibers, greatly improving the strength of the composite material. Summary of the invention

[0004] The purpose of the present invention is to provide a UHMWPE / HDPE composite material and a preparation method thereof in view of the problems existing in the application of existing UHMWPE in a polyolefin matrix. The method realizes the distribution and arrangement orientation of UHMWPE in a HDPE matrix by introducing a micro-nano stacking co-extrusion method, and is a new method for preparing a UHMWPE / HDPE composite material. The composite material prepared by the method contains oriented UHMWPE microfibers.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0006] A UHMWPE / HDPE composite material is prepared by using a micro-nano lamination extrusion device to extrude 100 parts by weight of high-density polyethylene (HDPE) and 10 to 50 parts by weight of ultra-high molecular weight polyethylene (UHMWPE) to form a multi-layer PE micro-layer structure arranged in parallel along the sheet extension direction, wherein UHMWPE fibers are arranged in an orderly manner along the extrusion direction.

[0007] The HDPE has a molecular weight of 200,000 to 500,000 and a melting point of 120 to 130°C.

[0008] The UHMWPE has a molecular weight of 2 million to 20 million and a melting point of 135 to 155°C.

[0009] Furthermore, the preparation method of the UHWPE / HDPE composite material comprises the following steps:

[0010] i) Mixing and drying: Add the required raw materials into the mixing unit according to the proportion, mix them evenly and dry them. The drying temperature of the raw materials is 80-100°C and the drying time is 60-120 minutes;

[0011] ii) the mixed raw materials are melt-blended and extruded through a twin-screw extruder and granulated to obtain a masterbatch, and the temperature of each section of the twin-screw extruder is set to 180° C., 190° C., 200° C., and 190° C. respectively;

[0012] iii) Cascading extrusion: The masterbatch obtained in step ii) is respectively fed into two extruders and a micro-nano cascading extrusion device composed of a cascading distributor, an expanding die, a diversion trough and a cutting machine. The mixed material is continuously divided and stacked in the layer distributor and subjected to a strong shear-stretching composite flow field. Finally, the composite melt is extruded from the die head under the extrusion action of the screw, wherein the temperature of the extruder body is 180-200°C, the temperature of the cascading distributor is 190-210°C, and the temperature of the die head is 190-200°C.

[0013] Step iii) The layer distributor is n stacking units connected in series. The composite melt is divided into m equal parts along the width direction at the inlet of the stacking unit. Each equal part continues to flow forward along the orientation die and rotates 90 degrees while expanding m times, and the thickness is reduced to 1 / m times. In this process, the HDPE and UHMWPE mixed melt forms a micro-layer film in the cavity due to the biaxial stretching effect, and converges into m layers of composite melt at the outlet and enters the next stacking unit; wherein n and m are integers not less than 2 respectively.

[0014] The stacked distributor is designed and processed according to the patent of Beijing University of Chemical Technology (Chinese patent 200910237622.5, US patent 3557265), and is a twisted stacked distributor.

[0015] The technical principle of the present invention is: to realize in-situ microfibrillation of UHMWPE dispersed phase in HDPE through micro-nano lamination co-extrusion equipment, and to obtain highly oriented UHMWPE reinforced HDPE material uniformly distributed along the longitudinal (MD) direction by utilizing the strong shear and stretching flow field in the laminator.

[0016] The present invention has the following beneficial effects:

[0017] 1. The in-situ microfibrillation of UHMWPE dispersed phase in HDPE is achieved through micro-nano lamination co-extrusion equipment. The strong shear and stretching flow field characteristics in the laminator are utilized to not only solve the problems of extremely high viscosity of UHMWPE melt, many physical entanglements of molecular chains, and difficulty in material processing, but also enable it to obtain highly oriented microfibrillated arrangement along the extrusion direction, thereby improving the strength of the composite material.

[0018] 2. The strong shear and tensile force field in the stacker can improve the crystallization performance and micromorphology of PE materials and enhance the orientation of PE molecular chains in the flow direction. At the same time, the melting point of UHMWPE is slightly higher than that of HDPE. The incompletely melted UHMWPE is fiberized at the interface between layers under the action of strong shear and tensile force fields, which is beneficial to further improve the mechanical strength of the composite material.

[0019] 3. This method uses micro-nano lamination technology to achieve uniform dispersion and oriented fiberization of UHMWPE in HDPE matrix materials, thereby improving the strength of the composite material. The preparation method is simple, the production efficiency is high, and continuous batch production is possible. The production efficiency is high and the production cost is low. The product can be used as a masterbatch to blend with other polymer materials. It has strong industrialization capabilities and broad market prospects. DETAILED DESCRIPTION

[0020] The following embodiments may enable those skilled in the art to better understand the present invention, but are not intended to limit the present invention in any form.

[0021] The UHMWPE used in the following embodiments of the present invention is GUR 5113 UHMWPE with a number average molecular weight of 3.7×10 6 g / mol, produced and provided by Ticona.

[0022] The HDPE used is HDPE5502, which is produced and provided by Shanghai Secco Petrochemical Co., Ltd.

[0023] The stacking distributor used is designed and processed according to the patent of Beijing University of Chemical Technology. It is a twisted stacking distributor, where n=3, m=4, and the extruded sheet contains 128 layers (2x4 3 =128). The composite melt is divided into 4 equal parts along the width direction at the inlet of the lamination unit, and each equal part continues to flow forward along the orientation die and rotates 90° while expanding 4 times, and the thickness is reduced to 1 / 4 times. In this process, the HDPE and UHMWPE mixed melt forms a microlayer film in the cavity due to the biaxial stretching effect, and converges into 4 layers of composite melt at the outlet and enters the next lamination unit.

[0024] Example 1

[0025] A method for preparing a UHWPE / HDPE composite material comprises the following steps:

[0026] 1) Weigh the following raw materials by weight:

[0027] HDPE 100 parts;

[0028] UHMWPE 10 parts;

[0029] 2) Mixing and drying: Add the required raw materials into the mixing unit according to the proportion, mix evenly and dry. The drying temperature of the raw materials is 80°C and the drying time is 120 minutes;

[0030] 3) The mixed raw materials are melt-blended and extruded through a twin-screw extruder and granulated to obtain a masterbatch, and the temperature of each section of the twin-screw extruder is set to 180°C, 190°C, 200°C, and 190°C respectively;

[0031] 4) Cascading extrusion: The masterbatch obtained in step 3) is respectively put into two extruders and a micro-nano cascading extrusion device composed of a cascading distributor, an expanding die, a diversion trough and a cutting machine. The mixed material is continuously divided and superimposed in the layer distributor and subjected to a strong shear-stretching composite flow field. Finally, the composite melt is extruded from the die head under the extrusion action of the screw, wherein the temperature of the extruder body is 190°C, the temperature of the cascading distributor is 200°C, and the temperature of the die head is 195°C.

[0032] Example 2

[0033] A method for preparing a UHWPE / HDPE composite material comprises the following steps

[0034] 1) Weigh the following raw materials by weight:

[0035] HDPE 100 parts;

[0036] UHMWPE 20 parts;

[0037] 2) Mixing and drying: Add the required raw materials into the mixing unit according to the proportion, mix evenly and dry. The drying temperature of the raw materials is 85°C and the drying time is 120 minutes;

[0038] 3) The mixed raw materials are melt-blended and extruded through a twin-screw extruder and granulated to obtain a masterbatch, and the temperature of each section of the twin-screw extruder is set to 180°C, 190°C, 200°C, and 190°C respectively;

[0039] 4. Layer extrusion: The masterbatch obtained in step 3) is respectively put into two extruders and a micro-nano layer extrusion device composed of a layer distributor, an expanding die, a diversion groove and a cutting machine. The mixed material is continuously divided and stacked in the layer distributor and subjected to a strong shear-stretch composite flow field. Finally, the melt is extruded from the die head under the extrusion action of the screw, wherein the temperature of the extruder body is 190°C, the temperature of the layer distributor is 200°C, and the temperature of the die head is 195°C.

[0040] Example 3

[0041] A method for preparing a UHWPE / HDPE composite material comprises the following steps

[0042] 1) Weigh the following raw materials by weight:

[0043] HDPE 100 parts;

[0044] UHMWPE 30 parts;

[0045] 2) Mixing and drying: Add the required raw materials into the mixing unit according to the proportion, mix evenly and dry. The drying temperature of the raw materials is 80°C and the drying time is 120 minutes;

[0046] 3) The mixed raw materials are melt-blended and extruded through a twin-screw extruder and granulated to obtain a masterbatch, and the temperature of each section of the twin-screw extruder is set to 180°C, 190°C, 200°C, and 190°C respectively;

[0047] 4) Cascading extrusion: The masterbatch obtained in step 3) is respectively put into two extruders and a micro-nano cascading extrusion device composed of a cascading distributor, an expanding die, a diversion trough and a cutting machine. The mixed material is continuously divided and stacked in the layer distributor and subjected to a strong shear-stretching composite flow field. Finally, the melt is extruded from the die head under the extrusion action of the screw, wherein the temperature of the extruder body is 190°C, the temperature of the cascading distributor is 200°C, and the temperature of the die head is 195°C.

[0048] Comparative Example 1

[0049] The formulation is the same as that of Example 1, and is directly blended and extruded into a sheet without passing through a laminating distributor.

[0050] Comparative Example 2

[0051] The formulation is the same as that of Example 2, and is directly blended and extruded into a sheet without passing through a laminating distributor.

[0052] Comparative Example 3

[0053] The formulation is the same as that of Example 3, but is directly blended and extruded into a sheet without passing through a laminating distributor.

[0054] Table 1 Comparison of composite materials components and properties

[0055]

[0056] As can be seen from the above table, in the examples, with the increase in the amount of UHMWPE added, the heat deformation temperature, tensile yield stress and notched impact strength of the composite material are significantly improved. In the comparative example, at a low UHMWPE addition (Comparative Example 1, 10 parts), the various properties are equivalent to those in Example 1, and with the increase in the amount of addition, the performance indicators do not change significantly. This result shows that under the action of the shear and tensile force field of the stacked distributor, the molecular chain entanglement behavior of UHMWPE is overcome, and the crystallization performance is improved. Compared with the commercially available HDPE5202 (tensile yield stress 27MPa, notched impact strength 12.7KJ / m 2 ), the mechanical strength of the composite material prepared by the embodiment of the present invention is unexpectedly improved, indicating that the composite material prepared by the method of the present invention contains oriented UHMWPE microfibers, which play a role of fiber reinforcement material to a certain extent.

[0057] The above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. Those skilled in the art should understand that the above specific descriptions are illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.

Claims

1. A UHMWPE / HDPE composite material, It is characterized in that It is prepared by micro-nano lamination extrusion equipment with 100 parts by weight of HDPE and 10 to 50 parts by weight of UHMWPE to form a multi-layer PE micro-layer structure arranged in parallel along the sheet extension direction, in which UHMWPE fibers are arranged in an orderly manner along the extrusion direction.

2. A method for preparing a UHMWPE / HDPE composite material according to claim 1, It is characterized in that The following steps are involved: i) Mixing and drying: Add the required raw materials into the mixing unit according to the proportion, mix evenly and dry. The drying temperature of the raw materials is 80~100℃ and the drying time is 60~120min; ii) the mixed raw materials are melt-blended and extruded through a twin-screw extruder and granulated to obtain a masterbatch, and the temperature of each section of the twin-screw extruder is set to 180° C., 190° C., 200° C., and 190° C. respectively; iii) Cascading extrusion: The masterbatch obtained in step ii) is respectively fed into two extruders and a micro-nano cascading extrusion device composed of a cascading distributor, an expanding die, a diversion trough and a cutting machine. The mixed material is continuously divided and superimposed in the layer distributor and subjected to a strong shear-stretching composite flow field. Finally, the composite melt is extruded from the die head under the extrusion action of the screw, wherein the temperature of the extruder body is 180-200°C, the temperature of the cascading distributor is 190-210°C, and the temperature of the die head is 190-200°C.

3. A method for preparing a UHMWPE / HDPE composite material according to claim 2, It is characterized in that Step iii) The layer distributor is composed of n stacking units connected in series. The composite melt is divided into m equal parts along the width direction at the inlet of the stacking unit. Each part continues to flow forward along the orientation die and rotates 90° while widening by m times, and the thickness is reduced to 1 / m times. During this process, the HDPE and UHMWPE mixed melt forms a microlayer film in the cavity due to the biaxial stretching effect, and converges into m layers of composite melt at the outlet and enters the next stacking unit; wherein n and m are integers not less than 2 respectively.

4. The method for preparing a UHMWPE / HDPE composite material according to claim 2, It is characterized in that The HDPE has a molecular weight of 200,000 to 500,000 and a melting point of 120 to 130°C.

5. The method for preparing a UHMWPE / HDPE composite material according to claim 2, It is characterized in that The UHMWPE has a molecular weight of 2 million to 20 million and a melting point of 135 to 155°C.

Citation Information

Patent Citations

  • Process for producing multilayered microporous polyolefin film

    CN101291794A

  • Micro-nano multi-layer composite dielectric materials and preparation method and device thereof

    CN103129070A

  • Heat-conducting PET (polyethylene terephthalate) film with laminated structure and preparation method of heat-conducting PET film

    CN117818185A

  • Laminate and packaging container using it

    JP2004284126A

  • Microlayer Structures and Methods

    US20080254281A1