Polylysine-titanium dioxide composite hydrogel as well as preparation method and application thereof
By using polylysine-titanium dioxide composite hydrogel under ultraviolet light, the problems of long curing time, insufficient mechanical properties and poor antibacterial properties are solved, and rapid curing and efficient antibacterial properties are achieved. Suitable for multiple application areas.
Patent Information
- Application Number
- CN202411064162.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-08
AI Technical Summary
The existing hydrogel preparation technology has problems such as long curing time, insufficient mechanical properties, complex operation and poor antibacterial properties, which limits its efficiency and breadth in industrial production and application.
The preparation method of polylysine-titanium dioxide composite hydrogel is adopted, and the rapid curing water is formed by using raw materials such as water, polylysine, nano-scale titanium dioxide, acrylamide, crosslinking agent and photoinitiator under ultraviolet light irradiation. Gel, improves mechanical properties and antibacterial properties.
It achieves rapid curing at room temperature (the curing time is shortened to less than 3 minutes), simplifies operating procedures, improves mechanical properties and antibacterial properties, and is suitable for the fields of biomedical and environmental protection, significantly improving production efficiency and application prospects.
Smart Images

Figure BDA0004978884110000051 
Figure BDA0004978884110000061 
Figure HDA0004978884130000011
Abstract
Description
Technical Field
[0001] The invention relates to a polylysine-titanium dioxide composite hydrogel and a preparation method and application thereof, belonging to the technical field of industrialized production of hydrogels. Background Art
[0002] As a polymer material with a three-dimensional network structure, hydrogel has been widely used in biomedicine, tissue engineering, environmental protection, cosmetics and other fields due to its unique physical and chemical properties. Existing hydrogel preparation methods mainly include chemical crosslinking and physical crosslinking. Chemical crosslinking usually involves the use of crosslinking agents to form covalent bonds between monomers or polymers, while physical crosslinking relies on non-covalent interactions such as hydrogen bonds and ionic interactions.
[0003] However, existing hydrogel preparation technologies have the following problems and limitations:
[0004] Long curing time: Traditional hydrogel preparation methods often require a long curing time, which limits production efficiency, especially in industrial production.
[0005] Insufficient mechanical properties: Many hydrogels have deficiencies in mechanical properties, such as low strength and poor toughness, which limits their application in certain fields.
[0006] Complex preparation process: Existing hydrogel preparation methods often involve multiple steps and complex operation processes, requiring specific equipment and conditions, which increases the technical threshold and operational difficulty.
[0007] Insufficient antibacterial properties: In fields such as biomedicine and environmental engineering, the antibacterial properties of hydrogels are an important consideration. However, existing hydrogels often lack effective antibacterial capabilities.
[0008] In response to the above problems, researchers have been looking for new ways to improve the preparation of hydrogels. In particular, the development of hydrogel preparation technology that can quickly solidify at room temperature, is easy to operate, and has excellent mechanical properties and antibacterial properties has always been a research hotspot in the field of industrial production of hydrogels. Summary of the invention
[0009] Purpose of the invention: The first purpose of the present invention is to provide a polylysine-titanium dioxide composite photopolymerized hydrogel with excellent antibacterial properties. The second purpose of the present invention is to provide a preparation method of the polylysine-titanium dioxide composite hydrogel that is rapidly solidified at room temperature, aiming to improve production efficiency, simplify the operation process, and enhance the mechanical properties of the hydrogel. The third purpose of the present invention is to provide the application of the polylysine-titanium dioxide composite hydrogel in the fields of biomedicine, environmental protection or tissue engineering.
[0010] Technical solution: The polylysine-titanium dioxide composite hydrogel described in the present invention includes water, polylysine, nano-sized titanium dioxide, acrylamide, a crosslinking agent and a photoinitiator as raw materials, and is solidified under ultraviolet light.
[0011] Furthermore, the molecular weight of the polylysine is 1023-5776 Daltons.
[0012] Furthermore, the polylysine consists of 7-35 lysine units.
[0013] Furthermore, the particle size of the nano-scale titanium dioxide is less than 5 nm.
[0014] Furthermore, the photoinitiator is 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, azobisisobutylamidine hydrochloride or azobisisobutylimidazoline hydrochloride, and the crosslinking agent is N,N'-methylenebisacrylamide or polyethylene glycol diacrylate.
[0015] Furthermore, the mass ratio of deionized water, polylysine, nano-sized titanium dioxide, acrylamide monomer, crosslinking agent and photoinitiator is 100:0.1-2:0.1-2:40-80:0.1-0.4:1-3, preferably 100:2:2:60:0.2:2.
[0016] The method for preparing the polylysine-titanium dioxide composite hydrogel of the present invention comprises the following steps:
[0017] (1) adding acrylamide monomer and a cross-linking agent into deionized water, stirring and dissolving, and obtaining a mixed solution;
[0018] (2) adding polylysine and nano-sized titanium dioxide to the mixed solution and continuing to stir to form a uniform dispersion;
[0019] (3) Adding a photoinitiator to the dispersion, stirring in a dark place, and curing the mixed dispersion under ultraviolet light.
[0020] Furthermore, in step (1), the stirring and dissolving time is more than 5 minutes.
[0021] Furthermore, in step (2), the stirring and dissolving time is continued for more than 5 minutes.
[0022] Furthermore, in step (3), the time of stirring in the dark is more than 20 minutes.
[0023] Furthermore, in step (3), the wavelength of the ultraviolet light is 250-420nm, and the intensity of the ultraviolet light is 3000-6000W.
[0024] Furthermore, in step (3), the curing time is within 3 minutes.
[0025] Application of the polylysine-titanium dioxide composite hydrogel of the present invention in the fields of biomedicine, environmental protection or tissue engineering.
[0026] The polylysine-titanium dioxide composite hydrogel obtained by the preparation method of the present invention not only has the characteristics of rapid curing, but also has excellent mechanical properties and antibacterial properties, and can effectively inhibit the growth of bacteria, such as Staphylococcus aureus and Escherichia coli. It can be used in various biomedical fields, environmental protection fields or tissue engineering and other fields, such as water pollution control, waste gas treatment, biomedicine, biomaterials, biomechanics, skin tissue engineering or bone tissue engineering. By introducing polylysine and nano-scale titanium dioxide, the present invention can improve the curing efficiency and performance of the hydrogel while simplifying the operation process, meeting the needs of industrial production.
[0027] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:
[0028] (1) Rapid preparation: The method of the present invention can shorten the curing time of the hydrogel from several hours to less than 3 minutes at room temperature, significantly improving production efficiency;
[0029] (2) Simple operation: The preparation process of the method of the present invention is simple, easy to control and operate, does not require complex equipment and conditions, and reduces the technical threshold and operation difficulty;
[0030] (3) Adjustable performance: The method of the present invention can achieve different functions and properties of the hydrogel by adjusting the raw material ratio and preparation conditions to meet the needs of different application fields;
[0031] (4) Excellent antibacterial properties: The polylysine-titanium dioxide composite hydrogel prepared by the method of the present invention can effectively inhibit bacterial growth and is suitable for the fields of biomedicine, environmental protection, etc.;
[0032] (5) Environmentally friendly: The photopolymerization method of the present invention reduces the use and emission of harmful chemicals, and is more environmentally friendly and sustainable;
[0033] (6) Broad application prospects: The method of the present invention is applicable to a variety of fields and has broad application prospects and market demands. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a graph showing the effect of polylysine with different molecular weights (degree of polymerization) on the curing time of hydrogel at room temperature in Example 1;
[0035] Figure 2This is a graph showing the effect of different amounts of polylysine with a polymerization degree of 25-35 and TiO2 with a particle size of 5 nm added together on the tensile properties of the hydrogel at room temperature in Example 2;
[0036] Figure 3 This is a test diagram of the antibacterial performance of the hydrogel in Example 3. DETAILED DESCRIPTION
[0037] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.
[0038] Poly-lysine was purchased from Zhejiang New Silver Elephant Bioengineering Co., Ltd., and the degrees of conjugation were 7-10, 11-24, and 25-35, i.e., the molecular weight ranges were 1023 -1562, 1854-3823, and 4130-5776 Daltons, respectively;
[0039] Staphylococcus aureus ST121 was purchased from Guangzhou Yangan Biotechnology Co., Ltd.;
[0040] Escherichia coli MG1655 was purchased from Shanghai Qincheng Biotechnology Co., Ltd.
[0041] Example 1
[0042] The effect of polylysine with different molecular weight (degree of polymerization) on the curing time of hydrogel at room temperature.
[0043] The hydrogel was prepared according to the following formula:
[0044] 1. Acrylamide (AAm): 60 g;
[0045] 2. Deionized water: 100g;
[0046] 3. N, N'-methylenebisacrylamide (MBA): 0.2 g;
[0047] 4. Photoinitiator: 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone: 2g;
[0048] 5. Polylysine: The polymerization degree of polylysine samples were 7-10, 11-24, and 25-35, i.e., the molecular weight ranges were 1023-1562, 1854-3823, and 4130-5776 Daltons, respectively, and the addition amount was 1 g;
[0049] 6. UV excitation wavelength and power: 400nm, 3000W;
[0050] 7. Temperature: room temperature (25℃).
[0051] First, add 60g of acrylamide monomer and 0.2g of N,N'-methylenebisacrylamide (MBA) cross-linker into a beaker. Subsequently, add 100g of deionized water and stir for 5 minutes to ensure that the monomer and cross-linker are completely dissolved. Next, add 1g of polylysine with different degrees of polymerization (the number of lysine units is 7-10, 11-24 and 25-35) to the solution respectively, and continue stirring for 5 minutes to form a uniform dispersion. After that, add 2g of photoinitiator 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone to the dispersion and stir in dark for 20 minutes until the photoinitiator is completely dissolved. The mixed dispersion is exposed to ultraviolet light with a power of 3000W and a wavelength of 400nm for curing to prepare a cured hydrogel. As a comparison, a hydrogel without the addition of polylysine was prepared using the same method as the control group (Null). See the specific effect of curing time. Figure 1 .
[0052] Figure 1 This is a graph showing the effect of polylysine with different molecular weights (degree of polymerization) on the curing time of hydrogel at room temperature in Example 1. Figure 1 The horizontal axis represents polylysine with different polymerization degrees added with 1g / 100mL water, and the vertical axis represents the curing time of the hydrogel; Null represents no polylysine added, P7-10 represents polylysine with a polymerization degree of 7-10; P11-24 represents polylysine with a polymerization degree of 11-24; and P25-35 represents polylysine with a polymerization degree of 25-35. Figure 1 The results show that polylysine with different molecular weights (degree of polymerization) has a significant effect on the curing of hydrogels. The curing time of hydrogels shortens as the molecular weight of polylysine increases. Polylysine with a degree of polymerization of 25-35 (molecular weight of 4130-5776 Daltons) performs best, shortening the curing time of hydrogels by 30% compared with the control group without polylysine.
[0053] Embodiment 2:
[0054] The effect of different addition amounts of polylysine with a degree of polymerization of 25-35 and TiO2 with a particle size of 5 nm on the curing time of hydrogel at room temperature.
[0055] The hydrogel was prepared according to the following formula:
[0056] 1. Acrylamide (AAm): 60 g;
[0057] 2. Deionized water: 100g;
[0058] 3. N, N'-methylenebisacrylamide (MBA): 0.2 g;
[0059] 4. Photoinitiator: 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone: 2g;
[0060] 5. Polylysine: Polylysine with a molecular weight of 4130-5776 Daltons, i.e., polylysine with a degree of polymerization of 25-35 lysine units, added in amounts of 0.5 g, 1 g, 1.5 g, and 2 g, respectively;
[0061] 6. Nano-TiO2: The particle size is 5nm TiO2, and the addition amounts are 0.5g, 1g, 1.5g and 2g respectively;
[0062] 7. UV light excitation wavelength and power: 400nm, 3000W;
[0063] 8. Temperature: room temperature (25℃).
[0064] First, 60g acrylamide (AAm) monomer and 0.2g N, N'-methylenebisacrylamide (MBA) cross-linking agent were added to a beaker. Then, 100g deionized water was added and stirred for 5 minutes to ensure that the monomer and cross-linking agent were completely dissolved. Next, the amount of polylysine added according to the degree of polymerization 25-35 (polylysine molecular weight is 4130-5776 Dalton) was 0.5g, 1 gram, 1.5g and 2g respectively; the amount of nano-TiO2 with a particle size of 5nm was added to the above solution in 0.5g, 1g, 1.5g and 2g respectively, and polylysine and nano-TiO2 were added to the above solution in equal amounts at the same time, and continued to stir for 5 minutes to form a uniform dispersion. Afterwards, 2 grams of photoinitiator 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone were added to the dispersion, and stirred for 20 minutes in dark until the photoinitiator was completely dissolved. Finally, the mixed dispersion was placed under ultraviolet light with a power of 3000W and a wavelength of 400nm for curing to prepare a cured hydrogel. For comparison, a hydrogel without adding polylysine and nano-TiO2 was prepared using the same method as a control group. The specific effects of curing time are shown in Table 1.
[0065] Table 1 Effect of polylysine and TiO2 on the curing time of hydrogel at room temperature
[0066]
[0067] Note: “Not added” means that neither poly-lysine nor titanium dioxide was added during the preparation of the hydrogel;
[0068] "P25-35" means polylysine with a degree of polymerization of 25-35; the TiO2 particle size used is 5nm; "P25-35 / TiO2" means that equal amounts of P25-35 and TiO2 with a particle size of 5nm are added at the same time.
[0069] It is obvious from the results of Table 1 that when the degree of polymerization is 25-35 of polylysine and the particle size is 5nm of TiO2 used in combination, their synergistic effect on the curing effect of hydrogel is more significant than when each is used alone. The experimental results show that when the addition amount of polylysine and TiO2 is 2g / 100ml water, the curing time of hydrogel is significantly shortened to less than 3 minutes from 26 minutes of the unadded group, which significantly improves the curing efficiency. Compared with our previously disclosed patent (CN118085166A), the curing time of TiO2 with a particle size of 5-10nm of 20g / 100ml water addition reported is 4 minutes. The research results in this patent have been improved in curing efficiency, further shortening the curing time to less than 3 minutes, and achieving a significant reduction in preparation cost. Specifically, the cost of using 20g of TiO2 with a particle size of 5-10nm is about 17 yuan, while the cost of using a combination of 2g of TiO2 with a particle size of 5nm and 2g of polylysine with a degree of polymerization of 25-35 is only about 3.8 yuan.
[0070] The hydrogel samples prepared in this example were cut into dumbbell shapes of 2×4×25 mm and subjected to tensile tests using a universal tensile testing machine (AGS). In the test, the tensile speed was set to 100 mm / min, aiming to evaluate the tensile properties of the hydrogel, including tensile strength, elongation at break, and fracture energy. During the test, the fracture energy of the hydrogel was calculated by integrating the area of the stress-strain curve. The specific results are as follows: Figure 2 And as shown in Table 2.
[0071] Table 2 Effect of 5 nanometer TiO2 addition on the physical properties of hydrogel under UV intensity of 3000W
[0072]
[0073] Note: The fracture energy and tensile strength in the table are obtained under the condition of maximum fracture elongation.
[0074] Figure 2 This is a graph showing the effect of different amounts of polylysine with a degree of polymerization of 25-35 and TiO2 with a particle size of 5 nm on the tensile properties of the hydrogel at room temperature in Example 2. Figure 2 The horizontal axis is tensile elongation, and the vertical axis is fracture energy; A) is a hydrogel with different concentrations of polylysine added; B) is a hydrogel with different concentrations of TiO2 added; C) is a hydrogel with equal amounts of polylysine and TiO2 added at the same time; the added concentrations of polylysine are 0.0g, 0.5g, 1.0g, 1.5g and 2.0g / 100ml water, respectively, with a degree of polymerization of 25-35, and the added concentrations of TiO2 are 0.0g, 0.5g, 1.0g and 2.0g / 100ml water, respectively, with a particle size of 5nm.
[0075] from Figure 2 It can be observed from the mechanical properties test results in Table 2 that with the increase in the amount of polylysine or TiO2 added, the fracture energy of the hydrogel gradually decreases, while the fracture elongation increases accordingly, which means that the flexibility of the hydrogel is enhanced. Specifically, when the addition amount of TiO2 is 2g / 100ml water, the fracture elongation of the hydrogel reaches 512% of the original length of the colloid, and the tensile strength is 74kPa; when the addition amount of polylysine is 1.5g / 100ml water, the fracture elongation reaches 628% of the original length of the colloid, and the tensile strength is 73kPa; and when polylysine and TiO2 are used in combination, each with an addition amount of 2g / 100ml water, the fracture elongation reaches 752% of the original length of the colloid, and the tensile strength reaches 97kPa. These data show that the combined use of polylysine and TiO2 can significantly improve the flexibility and tensile strength of the hydrogel.
[0076] Example 3
[0077] In this example, in order to evaluate the antibacterial properties of the hydrogel, the following experiments were performed:
[0078] (1) Preparation of bacterial strains: Take out Staphylococcus aureus (ST121,) and Escherichia coli (MG1655) from the -80°C refrigerator, streak culture on LB solid medium plates, and place in a 37°C incubator for 10 hours. Subsequently, pick a single colony and inoculate it into 5 ml LB liquid medium, and culture it at 37°C and 180 rpm for 12 hours.
[0079] (2) Preparation of bacterial solution: Centrifuge the cultured bacterial solution, discard the supernatant, wash the bacteria with sterile PBS buffer, and adjust the OD of the bacterial solution. 600 The value was adjusted to 0.6 to prepare a bacterial suspension.
[0080] (3) Preparation of hydrogel: The hydrogel using polylysine and TiO2 in Example 2 with addition amounts of 1.5 g / 100 ml water and 2 g / 100 ml water respectively.
[0081] (4) Antibacterial experiment: The prepared hydrogel was cut into discs with a diameter of 7 mm and immersed in sterile PBS buffer for 2 hours until saturated with water. The hydrogel disc after water absorption was placed on a 7 mm filter paper and then placed on an LB plate coated with 100 ul of bacterial suspension and cultured at 37°C for 12 hours. The formation of the antibacterial zone was observed and recorded.
[0082] The experimental results are as follows Figure 3 As shown, Figure 3The antibacterial performance test diagram of the hydrogel in Example 3, in which A) is the antibacterial experiment on Escherichia coli; B) is the antibacterial experiment on Staphylococcus aureus. The added concentration of polylysine group P25-35 is 1.5g / 100ml water, and the degree of polymerization is 25-35; the added concentration of TiO2 is 2.0g / 100ml water, and the particle size is 5nm; the concentrations of the two in the combined use group P25-35 / TiO2 are 1.5g / 100ml water and 2.0g / 100ml water respectively. The control group Control is a hydrogel without adding polylysine and TiO2. Figure 3 The experimental results show that the hydrogels using nano-titanium dioxide, polylysine or both alone show significant antibacterial effects, forming obvious antibacterial circles. And the antibacterial effect of the combined use of titanium dioxide and polylysine is significantly improved compared to the effect of using titanium dioxide or polylysine alone. This shows that the hydrogel of the present invention has good antibacterial properties and can effectively inhibit the growth of Staphylococcus aureus and Escherichia coli.
Claims
1. A polylysine-titanium dioxide composite hydrogel, characterized in that: The method comprises taking water, polylysine, nano-sized titanium dioxide, acrylamide, a cross-linking agent and a photoinitiator as raw materials and curing them under ultraviolet light.
2. The polylysine-titanium dioxide composite hydrogel according to claim 1, characterized in that: The molecular weight of the polylysine is 1023-5776 Daltons.
3. The polylysine-titanium dioxide composite hydrogel according to claim 2, characterized in that: The polylysine consists of 7-35 lysine units.
4. The polylysine-titanium dioxide composite hydrogel according to claim 1, characterized in that: The particle size of the nano-scale titanium dioxide is less than 5 nm.
5. The polylysine-titanium dioxide composite hydrogel according to claim 1, characterized in that: The photoinitiator is 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, azobisisobutylamidine hydrochloride or azobisisobutylimidazoline hydrochloride, and the crosslinking agent is N,N'-methylenebisacrylamide or polyethylene glycol diacrylate.
6. The polylysine-titanium dioxide composite hydrogel according to claim 1, characterized in that: The mass ratio of water, polylysine, nano-sized titanium dioxide, acrylamide monomer, cross-linking agent and photoinitiator is 100: 0.1-2: 0.1-2: 40-80: 0.1-0.4: 1-3.
7. The method for preparing the polylysine-titanium dioxide composite hydrogel according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) adding acrylamide monomer and a cross-linking agent into deionized water, stirring and dissolving, and obtaining a mixed solution; (2) adding polylysine and nano-sized titanium dioxide to the mixed solution and continuing to stir to form a uniform dispersion; (3) Adding a photoinitiator to the dispersion, stirring in a dark place, and curing the mixed dispersion under ultraviolet light.
8. The preparation method according to claim 7, characterized in that: In step (1), the stirring and dissolving time is more than 5 minutes, in step (2), the stirring and dissolving time is continued for more than 5 minutes, and in step (3), the stirring time in the dark is more than 20 minutes.
9. The preparation method according to claim 7, characterized in that: In step (3), the wavelength of the ultraviolet light is 250-420nm, the intensity of the ultraviolet light is 3000-6000W; and the curing time is within 3 minutes.
10. Use of the polylysine-titanium dioxide composite hydrogel according to any one of claims 1 to 6 in the fields of biomedicine, environmental protection or tissue engineering.
Citation Information
Cited By
Microbial composite hydrogel as well as preparation method and application thereof
CN119591256A
A microbial composite hydrogel, its preparation method and application
CN119591256B