Polypropylene insulating material based on chain modification as well as preparation method and application thereof
Through the chemical reaction of polypropylene and maleic anhydride graft modified polypropylene and diamino compounds, the problem of low melt viscosity of polypropylene insulating materials at low shear frequency is solved, and the viscosity and tensile characteristics of the material are improved. The insulation eccentricity problem is solved and the high voltage level application of polypropylene cables is realized.
Patent Information
- Application Number
- CN202411066330.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-08
AI Technical Summary
Polypropylene insulating materials with long straight molecular chain characteristics have low melt viscosity at low shear frequency, which leads to melt deformation and insulation eccentricity problems during cable processing and forming or when short-circuit thermal shock, limiting polypropylene The development of cables towards large insulation thickness and high voltage levels.
By mixing polypropylene with maleic anhydride graft modified polypropylene, diamino compounds and antioxidants, melt blending and hot-pressing molding, the polypropylene molecular chain is achieved by using the chemical reaction between the anhydride functional group and the amino group. Branching and reconstruction to enhance the viscosity and tensile properties of the material.
The viscosity, stress-strain characteristics and DC properties of polypropylene materials are significantly improved, effectively suppressing the insulation eccentricity problem caused by low zero-shear viscosity of the melt, and improving the material's electrical strength and tensile characteristics.
Smart Images

Figure CN118909385A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of polypropylene, and in particular to a polypropylene insulating material based on chain modification, and a preparation method and application thereof. Background Art
[0002] In recent years, green and environmental protection concepts have gradually become the main goals of social development. Thermoplastic polypropylene has environmentally friendly and recyclable characteristics and excellent electrical properties. Compared with cross-linked polyethylene (XLPE) insulated power cables, polypropylene cables do not require cross-linking and degassing during production, which reduces production cycles and energy consumption. Therefore, polypropylene is considered to be a new generation of cable insulation materials. However, polypropylene insulation materials with long straight molecular chains have low melt viscosity at low shear frequencies. During the cable processing and molding process or when the cable is subjected to short-circuit thermal shock, melt deformation and insulation eccentricity problems are prone to occur, which limits the development of polypropylene cables to large insulation thickness and high voltage levels. Summary of the invention
[0003] Based on this, it is necessary to provide a chain-modified polypropylene insulation material, which can improve the viscosity, tensile properties and DC performance of the polypropylene material, and can effectively suppress the eccentricity problem caused by the low zero-shear viscosity of the melt during the molding process of polypropylene cable insulation or when it is subjected to short-circuit thermal shock.
[0004] The technical solution is as follows:
[0005] One aspect of the present invention provides a chain-modified polypropylene insulating material, wherein the raw materials include the following components by weight: 0-50 parts of polypropylene, 0.1-100 parts of maleic anhydride grafted modified polypropylene, 0.5-4 parts of diamino compounds, and 0.3-1.5 parts of antioxidants.
[0006] In one embodiment, the diamino compound includes 3,3'-diaminodipropylamine.
[0007] In one embodiment, the active ingredient in the 3,3'-diaminodipropylamine is higher than 98%.
[0008] In one embodiment, the maleic anhydride grafted modified polypropylene is one or more of maleic anhydride grafted modified homopolypropylene or maleic anhydride grafted modified copolymer polypropylene; and / or
[0009] In the maleic anhydride grafted modified polypropylene, the grafting rate of maleic anhydride is 1%-3%.
[0010] In one embodiment, the polypropylene is one or more of homopolymer polypropylene or copolymer polypropylene.
[0011] In one embodiment, the antioxidant is one or more of antioxidant 1010 , antioxidant 1035 , antioxidant 1024 or antioxidant 300 .
[0012] In one of the embodiments, the raw materials of the polypropylene insulation material include the following components by weight: 0-50 parts of polypropylene, 0.1-100 parts of maleic anhydride grafted modified polypropylene, 0.5-1.5 parts of diamino compounds, and 0.3-1.5 parts of antioxidants.
[0013] Another aspect of the present invention provides a method for preparing the chain-modified polypropylene insulating material as described above, characterized in that it comprises the following steps:
[0014] The polypropylene, maleic anhydride grafted modified polypropylene, diamino compound and antioxidant are mixed, and the obtained mixture is melt blended and hot pressed into shape.
[0015] In one embodiment, the step of melt blending satisfies at least one of the following conditions:
[0016] (1) Temperature is 180℃-200℃;
[0017] (2) The speed is 40r / min-60r / min;
[0018] (3) Duration is 10-20 minutes; and / or
[0019] The step of hot pressing meets at least one of the following conditions:
[0020] (1) Temperature is 160℃-200℃;
[0021] (2) The pressure is 12MPa-18MPa.
[0022] In another aspect of the present invention, there is provided use of the chain-modified polypropylene cable insulation material as described above in preparing an insulation layer of a cable.
[0023] Compared with the prior art, this application has the following beneficial effects:
[0024] The present application provides a polypropylene material based on chain modification, which reconstructs the polypropylene macromolecular chain through a chemical reaction between the anhydride functional group on the polypropylene macromolecular chain modified by maleic anhydride grafting and the small molecule compound containing an amino group at the added end group, thereby improving the branching degree and molecular weight of the material, thereby improving the viscosity, stress-strain characteristics, DC resistivity and electrical strength of the polypropylene material, and improving the tensile properties and DC performance of the material. The material is applied to the insulation layer material of a power cable, and can effectively suppress the eccentricity problem caused by the low zero shear viscosity of the melt during the molding process of the polypropylene cable insulation or when it is subjected to short-circuit thermal shock. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0026] Figure 1 A graph of melt index and viscosity test results for different materials prepared for this application.
[0027] Figure 2 Figure 2. Stress-strain test results of different materials prepared for this application.
[0028] Figure 3 Volume resistivity and DC breakdown strength graph of different materials prepared for this application. DETAILED DESCRIPTION
[0029] The present application will be further described in detail below in conjunction with specific embodiments. The present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thoroughly understood.
[0030] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0031] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:
[0032] As used herein, "one or more" refers to any one, any two, or any two or more of the listed items.
[0033] Herein, the optional scope of "and / or", "or / and", and "and / or" includes any one of two or more related listed items, and also includes any and all combinations of related listed items, and the said any and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. It should be noted that when at least three items are connected by at least two conjunctions selected from "and / or", "or / and", and "and / or", it should be understood that in this application, the technical solution undoubtedly includes technical solutions that are all connected by "logical and", and undoubtedly includes technical solutions that are all connected by "logical or". For example, "A and / or B" includes three parallel solutions of A, B and A+B. For example, the technical solution of "A, and / or, B, and / or, C, and / or, D" includes any one of A, B, C, and D (that is, the technical solution that is all connected by "logical OR"), and also includes any and all combinations of A, B, C, and D, that is, the combination of any two or any three of A, B, C, and D, and also includes the combination of four of A, B, C, and D (that is, the technical solution that is all connected by "logical AND").
[0034] Herein, "further", "further", "particularly" and the like are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of this application.
[0035] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0036] The percentage contents involved in this application, unless otherwise specified, refer to mass percentage for solid-liquid mixing and solid-solid mixing, and refer to volume percentage for liquid-liquid mixing.
[0037] The percentage concentrations mentioned in this application, unless otherwise specified, refer to the final concentration, which refers to the percentage of the added component in the system after the addition of the component.
[0038] The temperature parameters in this application, unless otherwise specified, allow both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±2°C, ±1°C, ±0.5°C, ±0.4°C, ±0.3°C, ±0.2°C, and ±0.1°C are allowed. Normal temperature or room temperature in this application refers to no temperature control operation, generally 4°C~35°C, preferably 20±5°C.
[0039] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0040] The melt viscosity of polypropylene insulation materials with straight molecular chain characteristics is low at low shear frequencies, and melt deformation and insulation eccentricity problems are prone to occur during the cable processing and molding process or when the cable is subjected to short-circuit thermal shock, which limits the development of polypropylene cables to large insulation thickness and high voltage levels. Based on this, the present application provides a polypropylene material based on grafting modification and chain reconstruction, which is made of polypropylene maleic anhydride grafted modified polypropylene, diamino compounds, and antioxidants through melt blending. The branching and reconstruction of the polypropylene molecular chain are achieved through the chemical reaction between the anhydride functional group and the amino group, which can greatly improve the tensile strength and melt viscosity of the polypropylene material, and maintain DC performance similar to that of the polypropylene material.
[0041] One aspect of the present invention provides a chain-modified polypropylene insulating material, wherein the raw materials include the following components by weight: 0-50 parts of polypropylene, 0.1-100 parts of maleic anhydride grafted modified polypropylene, 0.5-4 parts of diamino compounds, and 0.3-1.5 parts of antioxidants.
[0042] In some examples, the diamino compound includes 3,3'-diaminodipropylamine.
[0043] In some of the examples, the active ingredient content of the 3,3'-diaminodipropylamine is higher than 98%.
[0044] In some examples, the maleic anhydride grafted modified polypropylene is one or more of maleic anhydride grafted modified homopolypropylene or maleic anhydride grafted modified copolymer polypropylene.
[0045] In some of the examples, the grafting rate of maleic anhydride in the maleic anhydride grafted modified polypropylene is 1%-3%. Specifically, the grafting rate refers to the mass percentage, and the grafting rate is limited to ensure that the material has sufficient chain modification sites and satisfies the maleic anhydride grafted modified polypropylene produced under the existing grafting process conditions. It can be understood that the grafting rate of the maleic anhydride grafted modified polypropylene includes but is not limited to 0.5%, 0.7%, 0.9%, 1.1%, 1.3%, and 1.5%.
[0046] In some examples, the polypropylene is one or more of homopolypropylene or copolymer polypropylene.
[0047] In some examples, the antioxidant is one or more of antioxidant 1010 , antioxidant 1035 , antioxidant 1024 , or antioxidant 300 .
[0048] In some of the examples, the raw materials of the chain-modified polypropylene insulation material include the following components by weight: 0-50 parts of polypropylene, 0.1-100 parts of maleic anhydride grafted modified polypropylene, 0.5-2 parts of diamino compounds, and 0.3-1.5 parts of antioxidants.
[0049] In some specific examples, the raw materials of the chain-modified polypropylene insulation material include the following components by weight: 0-50 parts of polypropylene, 50-100 parts of maleic anhydride grafted modified polypropylene, 0.5-2 parts of diamino compounds, and 0.3-1.0 parts of antioxidants.
[0050] In some specific examples, the raw materials of the chain-modified polypropylene insulation material include the following components by weight: 0-50 parts of polypropylene, 50-100 parts of maleic anhydride grafted modified polypropylene, 0.5-1.5 parts of diamino compounds, and 0.3-1.0 parts of antioxidants.
[0051] In some specific examples, the principles of chain-modified polypropylene insulation to achieve adhesion enhancement are as follows:
[0052] In the present application, maleic anhydride grafted polypropylene is used as a key component of a polypropylene insulating material. Since the maleic anhydride group carried by the maleic anhydride grafted polypropylene is easy to chemically react with the amino group of 3,3'-diaminodipropylamine to form a covalent bond, 3,3'-diaminodipropylamine having amino groups at both end groups is used as a viscosity-increasing reactant. In a molten state, the amino groups at both ends of the maleic anhydride grafted polypropylene will form a covalent bond with the maleic anhydride group on the polypropylene side group, thereby increasing the branching degree and molecular weight of the polypropylene macromolecule, thereby achieving viscosity-increasing of the polypropylene material.
[0053] At present, in the polypropylene synthesis process based on the Ziegler-Natta catalyst system, due to the limitation of the average lifespan of the growing macromolecular chains, secondary active centers cannot be formed and polypropylene materials with rich branching cannot be effectively synthesized. Therefore, its viscosity and melt strength are often low. Once the temperature is higher than the crystallization melting temperature of polypropylene, the polypropylene material cannot withstand large stress, which will cause deformation of the insulation structure in the cable. In order to improve the melt viscosity of polypropylene, there are currently mainly direct polymerization, irradiation, micro-crosslinking and blending modification methods, among which the direct polymerization method is to graft and polymerize various olefins with propylene during the polymerization of polypropylene. This method requires special initiators, huge one-time investment in production equipment, and difficult process research and development. At present, the technology is mainly monopolized by large foreign material suppliers; both irradiation and micro-crosslinking methods inevitably cause the degradation of polypropylene materials, resulting in aging of the materials and decreased insulation performance, which are not suitable for cable insulation; blending modification is a flexible, simple and effective viscosity modification method, which usually blends low melting temperature, highly branched structure or high molecular weight elastomers with polypropylene. Although the viscosity enhancement effect is significant, the elastomer also introduces a large number of interfaces in the polypropylene blend material. Due to the significant differences in electrical, thermal and mechanical properties between the two phases, for cable insulation, under the action of long-term electrical, thermal and force fields, defects are very likely to occur at the interface, resulting in degradation of cable insulation performance. Based on this, another aspect of the present invention provides a method for preparing a polypropylene insulation material based on chain modification as described above, comprising the following steps:
[0054] The polypropylene, maleic anhydride grafted modified polypropylene, diamino compound and antioxidant are mixed, and the obtained mixture is melt blended and hot pressed into shape.
[0055] In some examples, the conditions of the melt blending step include: a temperature of 180° C.-200° C. It can be understood that the temperature of the melt blending includes but is not limited to 180° C., 185° C., 190° C., 195° C., and 200° C.
[0056] In some examples, the conditions of the melt blending step include: a rotation speed of 40 r / min-60 r / min. It can be understood that the rotation speed of the melt blending step includes but is not limited to 40 r / min, 45 r / min, 50 r / min, 55 r / min, and 60 r / min.
[0057] In some of the examples, the conditions of the melt blending step include: a time of 10 min-20 min. It can be understood that the time of melt blending includes but is not limited to 10 min, 12 min, 14 min, 15 min, 18 min, 20 min.
[0058] In some examples, the conditions of the step of thermoforming include: a temperature of 160° C.-200° C. It can be understood that the temperature of thermoforming includes but is not limited to 160° C., 170° C., 180° C., 190° C., and 200° C.
[0059] In some examples, the conditions of the hot pressing step include: a pressure of 12 MPa-18 MPa. It can be understood that the pressure of hot pressing includes but is not limited to 12 MPa, 13 MPa, 14 MPa, 15 MPa, 16 MPa, 17 MPa, and 18 MPa.
[0060] In another aspect of the present invention, there is provided use of the chain-modified polypropylene cable insulation material as described above in preparing an insulation layer of a cable.
[0061] The following is further described in conjunction with specific embodiments. The raw materials involved in the following specific embodiments, unless otherwise specified, can all be commercially available; the instruments used, unless otherwise specified, can all be commercially available; the processes involved, unless otherwise specified, are all routinely selected by those skilled in the art.
[0062] The following are specific embodiments.
[0063] Example 1
[0064] This embodiment provides a chain-modified tackifying polypropylene insulation material, which is prepared by melt blending components in the following proportions:
[0065] Maleic anhydride grafted modified copolymer polypropylene (grafting rate 1%) 100 parts;
[0066] 1.0 part of 3,3'-diaminodipropylamine;
[0067] Antioxidant 1010 0.5 parts.
[0068] The specific preparation method of the chain-modified tackifying polypropylene insulating material provided in this embodiment includes the following steps:
[0069] The grafted modified copolymer polypropylene, 3,3'-diaminodipropylamine and antioxidant were uniformly mixed in proportion, the resulting mixture was melt blended at 190°C and 60r / min for 10 minutes, and the obtained viscosity-enhanced polypropylene insulation material was hot-pressed in a flat vulcanizer at 180°C and 15MPa, and vacuum-dried after cooling to obtain a viscosity-enhanced polypropylene insulation sample (PP-1).
[0070] Example 2
[0071] This embodiment provides a chain-modified tackifying polypropylene insulation material, which is prepared by melt blending components in the following proportions:
[0072] Maleic anhydride grafted modified copolymer polypropylene (grafting rate 1%) 100 parts;
[0073] 1.5 parts of 3,3'-diaminodipropylamine;
[0074] Antioxidant 1010 0.5 parts.
[0075] The specific preparation method of the chain-modified tackifying polypropylene insulating material provided in this embodiment includes the following steps:
[0076] The grafted modified copolymer polypropylene, 3,3'-diaminodipropylamine and antioxidant were uniformly mixed in proportion, the resulting mixture was melt blended at 190°C and 60r / min for 10 minutes, and the obtained viscosity-enhanced polypropylene insulation material was hot-pressed in a flat vulcanizer at 180°C and 15MPa, and vacuum-dried after cooling to obtain a viscosity-enhanced polypropylene insulation sample (PP-2).
[0077] Example 3
[0078] This embodiment provides a chain-modified tackifying polypropylene insulation material, which is prepared by melt blending components in the following proportions:
[0079] Maleic anhydride grafted modified copolymer polypropylene (grafting rate 1%) 100 parts;
[0080] 2.0 parts of 3,3'-diaminodipropylamine;
[0081] Antioxidant 1010 0.5 parts.
[0082] The specific preparation method of the chain-modified tackifying polypropylene insulating material provided in this embodiment includes the following steps:
[0083] The grafted modified copolymer polypropylene, 3,3'-diaminodipropylamine and antioxidant were uniformly mixed in proportion, the resulting mixture was melt blended at 190°C and 60r / min for 10 minutes, and the obtained viscosity-enhanced polypropylene insulation material was hot-pressed in a flat vulcanizer at 180°C and 15MPa, and vacuum-dried after cooling to obtain a viscosity-enhanced polypropylene insulation sample (PP-3).
[0084] Example 4
[0085] This embodiment provides a chain-modified tackifying polypropylene insulation material, which is prepared by melt blending components in the following proportions:
[0086] Polypropylene 50 parts;
[0087] Maleic anhydride grafted modified copolymer polypropylene (grafting rate 1.5%) 50 parts;
[0088] 2.0 parts of 3,3'-diaminodipropylamine;
[0089] Antioxidant 1010 0.5 parts.
[0090] The specific preparation method of the chain-modified tackifying polypropylene insulating material provided in this embodiment includes the following steps:
[0091] Polypropylene, grafted modified copolymer polypropylene, 3,3'-diaminodipropylamine and antioxidant were uniformly mixed in proportion, the resulting mixture was melt blended at 190°C and 60r / min for 10 minutes, and the obtained viscosity-enhanced polypropylene insulation material was hot-pressed in a flat vulcanizer at 180°C and 15MPa, and vacuum-dried after cooling to obtain a viscosity-enhanced polypropylene insulation sample (PP-4).
[0092] Comparative Example 1
[0093] This comparative example provides a polypropylene insulation material, which is prepared by melt blending the following components:
[0094] 100 parts of copolymerized polypropylene;
[0095] Antioxidant 1010 0.3 parts.
[0096] The specific preparation method steps of the chain-modified tackifying polypropylene insulating material provided in this comparative example are as follows:
[0097] The copolymerized polypropylene and the antioxidant were uniformly mixed in proportion, the obtained mixture was melt blended at 190°C and 60r / min for 10min, and the obtained polypropylene insulation material was hot-pressed in a flat vulcanizer at 180°C and 15MPa, and vacuum dried after cooling to obtain a polypropylene insulation sample (PP).
[0098] Comparative Example 2
[0099] This comparative example provides a polypropylene insulation material, which is prepared by melt blending the following components:
[0100] Maleic anhydride grafted modified copolymer polypropylene (grafting rate 2%) 100 parts;
[0101] Antioxidant 1010 0.3 parts.
[0102] The specific preparation method of the chain-modified tackifying polypropylene insulating material provided in this comparative example is as follows:
[0103] The grafted modified copolymer polypropylene and the antioxidant were uniformly mixed in proportion, the resulting mixture was melt blended at 190°C and 60r / min for 10min, and the obtained polypropylene insulation material was hot-pressed in a flat vulcanizer at 180°C and 15MPa, and vacuum dried after cooling to obtain a polypropylene insulation sample (PPg).
[0104] The polypropylene insulation materials prepared in Examples 1 to 4 and Comparative Examples 1 to 2 were tested for rheological properties, stress-strain properties, DC resistivity and electrical strength performance, and the test results are as follows.
[0105] 1. Rheological properties
[0106] Figure 1 The results of the melt index and viscosity test are shown in Figure 2. The rotational rheology test temperature is 200°C, and the shear rate corresponding to the low shear viscosity is 0.05 rad / s. Figure 1 It can be seen that the low shear viscosity of pure PP is 17400 Pa·s; while the grafted modified PP material slightly decreases to 14300 Pa·s due to the β-degradation of the macromolecular chain caused by the free radical process initiated by the initiator; with the increase of the amount of small molecule compounds that can achieve bridging, the low shear viscosity increases from 17400 Pa·s to 31800 Pa·s, and the viscosity increase rate reaches 82.75% at low shear rate.
[0107] The melt index test refers to ASTM1238 standard, the test conditions are 230℃, 2.16kg, and the mass of the standard aperture extruded material is recorded for 10 minutes. The test results are as follows Figure 1 As shown in the figure, the melt index of the viscosity-enhanced polypropylene after molecular chain reconstruction has dropped significantly, and the extent of the drop is positively correlated with the amount of diamino small molecule compound added, which is consistent with the low shear viscosity test results.
[0108] 2. Stress-strain characteristics
[0109] Figure 2 The stress-strain test results of different materials are shown in FIG. 1. The samples prepared in Example 1, Example 2, Example 3 and Comparative Example 1 and Comparative Example 2 are punched into standard dumbbell-shaped samples, and stress-strain tests are performed according to the standard of GB / T1040.2-2006, with a tensile speed of 50 mm / min. Figure 2 It can be seen that the tensile properties of PP materials slightly decreased before and after grafting modification, which is related to the degradation of PP macromolecular chains during the grafting reaction. The yield strength of the four thickening PP materials was significantly improved, the cold drawing section was significantly extended, and the slope of the curve in the later strain hardening stage was greatly improved, indicating that the introduction of bridging bonds increased the branching degree and molecular weight of the material, which significantly improved the tensile strength and elongation at break of the thickening material.
[0110] (III) DC resistivity and dielectric strength
[0111] The samples prepared in Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2 were subjected to DC resistivity and dielectric strength tests. The DC resistivity test was conducted at room temperature, using a three-electrode system, and the sample was polarized for 30 minutes at an electric field strength of 20 kV / mm, and then the conduction current flowing through the sample was read to calculate the DC resistivity of the material; the dielectric strength test was conducted at a voltage increase rate of 0.5 V / s, with a sample thickness of 0.1 mm, until the sample broke down, and the breakdown field strength of each sample was processed based on the Weibull distribution to obtain the dielectric strength of the material.
[0112] from Figure 3 It can be seen that the DC resistivity of the grafted modified and thickened PP material is increased by nearly one order of magnitude compared with PP. The deep traps generated by the introduction of various polar groups (carbonyl, amino) in the material limit the carrier migration and inhibit the conductive current flowing through the sample under the polarization electric field, thereby increasing the DC resistivity of the material. However, the DC resistivity of Example 3 with a high addition content is slightly lower than that of Examples 1 and 2. This may be due to the increase in the density of polar groups, which causes the electron cloud distribution to overlap and weakens the trap energy level introduced by the polar groups.
[0113] The electrical strength of the six materials are all higher than 300kV / mm, and they have excellent electrical insulation properties. The electrical strength of the PPg material is slightly higher than that of PP. The DC performance of the diluted PP-4 is slightly improved compared with that of PP-2, while the electrical strength of the three thickening polypropylene materials is slightly lower than that of PP. This is because amino groups that attract holes are further introduced into the PPg material. The interaction between the amino group and the carbonyl group causes the energy level of the electron trap introduced by the carbonyl group to decrease. At the same time, the hole trap has a weaker ability to restrict electrons, which weakens the constraint and dissipation effect of the trap on high-energy electrons, resulting in a slight decrease in the electrical strength.
[0114] Considering the viscosity, tensile properties and DC performance of the material, although the electrical strength of the material decreases slightly after viscosity increase, this modification method has a significant improvement effect on the rheological extrusion properties of the material. At the same time, its DC performance meets the needs of the working conditions. Therefore, the viscosity-increased polypropylene insulation material proposed in the present invention is of great significance for the further development of polypropylene insulated cable insulation.
[0115] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0116] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims, and the description may be used to interpret the content of the claims.
Claims
1. A polypropylene insulation material based on chain modification, characterized in that, The raw materials include the following components by weight: 0-50 parts of polypropylene, 0.1-100 parts of maleic anhydride grafted modified polypropylene, 0.5-4 parts of diamino compounds, and 0.3-1.5 parts of antioxidants.
2. The chain-modified polypropylene insulation material according to claim 1, characterized in that The diamino compound includes 3,3'-diaminodipropylamine.
3. The chain-modified polypropylene insulation material according to claim 2, characterized in that The effective component of the 3,3'-diaminodipropylamine is higher than 98%.
4. The chain-modified polypropylene insulation material according to claim 1, characterized in that The maleic anhydride grafted modified polypropylene is one or more of maleic anhydride grafted modified homopolypropylene or maleic anhydride grafted modified copolymer polypropylene; and / or In the maleic anhydride grafted modified polypropylene, the grafting rate of maleic anhydride is 1%-3%.
5. The chain-modified polypropylene insulation material according to claim 1, characterized in that The polypropylene is one or more of homopolypropylene and copolymer polypropylene.
6. The chain-modified polypropylene insulation material according to claim 1, characterized in that The antioxidant is one or more of antioxidant 1010 , antioxidant 1035 , antioxidant 1024 or antioxidant 300 .
7. The chain-modified polypropylene insulation material according to any one of claims 1 to 6, characterized in that: The raw materials include the following components by weight: 0-50 parts of polypropylene, 0.1-100 parts of maleic anhydride grafted modified polypropylene, 0.5-1.5 parts of diamino compounds, and 0.3-1.5 parts of antioxidants.
8. A method for preparing a chain-modified polypropylene insulating material according to any one of claims 1 to 7, characterized in that: The steps include: The polypropylene, maleic anhydride grafted modified polypropylene, diamino compound and antioxidant are mixed, and the obtained mixture is melt blended and hot pressed into shape.
9. The chain-modified polypropylene insulation material according to claim 8, characterized in that The step of melt blending satisfies at least one of the following conditions: (1) Temperature is 180℃-200℃; (2) The speed is 40r / min-60r / min; (3) Duration is 10-20 minutes; and / or The step of hot pressing meets at least one of the following conditions: (1) Temperature is 160℃-200℃; (2) The pressure is 12MPa-18MPa.
10. Use of the chain-modified polypropylene cable insulation material according to any one of claims 1 to 7 in preparing an insulation layer of a cable.
Citation Information
Patent Citations
Preparation method of cable insulating layer material with polyolefin-grafted polar groups
CN105949394A
High-melt-strength polypropylene as well as preparation method and application thereof
CN112080100A
Application of anhydride group-containing polypropylene graft as insulating material and insulating material
CN113563520A
Method for producing polar group-containing polyolefin
JP2019081897A
Polymers obtained from oligomers of anhydride-grafted polypropylene, manufacturing process and uses
US4735992A
Cited By
Method for improving breakdown strength and uniformity of biaxially oriented polypropylene film by using nitrogen-oxygen mixed plasma
CN122034363A