Low-density epoxy resin and preparation method thereof

By first adding thickener and accelerator to the epoxy resin, combined with hydrophilic aerogel filler, the problems of high density and insufficient thermal insulation performance of traditional metal materials are solved, and low density, high mechanical properties and low thermal conductivity are prepared. The coefficient of epoxy resin material achieves lightweight and environmentally friendly production.

CN118909397APending Publication Date: 2024-11-08GONGSHENG (TIANJIN) NEW MATERIAL TECH PARTNERSHIP (LLP)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410908233.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Traditional metal materials have shortcomings in reducing density and improving mechanical properties and thermal insulation properties, which are particularly difficult to meet the needs of lightweight at the same time. The traditional epoxy resin addition method is not suitable for fillers with fluffy porous structures.

Method used

Using low-density heat-insulating epoxy resin, the viscosity is increased by adding thickener and accelerator to the epoxy resin to reduce the mixing rate of the resin and high specific area filler, and hydrophilic gas condensation under low viscosity conditions Glue filler to reduce material density while using epoxy resin wetting agent and diluent to reduce thermal conductivity.

Benefits of technology

The preparation of low-density (1.05-1.15g/cm3), high mechanical properties and low thermal conductivity (0.14-0.16) materials is achieved, which reduces the material density and improves the thermal insulation performance, while avoiding the use of volatile substances and VOCs. Emissions improve environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure BDA0004932781670000011
    Figure BDA0004932781670000011
Patent Text Reader

Abstract

The invention relates to low-density heat-insulating epoxy resin and a preparation method thereof.The low-density heat-insulating epoxy resin is prepared from, by weight, 90-110 parts of epoxy resin, 2-20 parts of curing agent, 1-8 parts of accelerant, 1-10 parts of auxiliaries, 2-10 parts of thickening agent and 2-5 parts of filler, the thickening agent is added into the epoxy resin firstly, so that the viscosity of the epoxy resin is increased, permeation of the resin to aerogel micropores is reduced, and the heat-insulating property of the epoxy resin is improved; according to the low-density heat-insulating epoxy resin, the porous structure is prevented from being tamped, then the filler (aerogel) is added, the density of the material is effectively reduced by the porous loose structure from 1.2 g / cm < 3 > to 1.1 g / cm < 3 >, the low-density heat-insulating epoxy resin does not contain volatile substances during production, VOC emission is avoided in the production process, and the low-density heat-insulating epoxy resin is more environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a low-density epoxy resin and a preparation method thereof. Background Art

[0002] With the development of high-speed rail and automobile industries, the demand for lightweighting is getting higher and higher, especially in reducing material density, improving material mechanical properties and thermal insulation performance. Traditional metal materials cannot achieve these properties at the same time. Therefore, it is urgent to develop a new type of thermosetting material that meets the requirements of low density, high mechanical properties and low thermal conductivity.

[0003] The traditional epoxy resin adding method is to add epoxy resin and filler first, and then add thickener to ensure that it is evenly mixed with filler under low viscosity conditions to facilitate the infiltration of filler. However, this method is not suitable for fillers with fluffy porous structures. Summary of the invention

[0004] In order to solve the above technical problems, the present invention is proposed. The present invention provides a low-density epoxy resin and a preparation method thereof, which solves the technical problem of high density of thermosetting materials in the prior art.

[0005] According to the first aspect of the present application, the present invention provides a low-density thermal insulation epoxy resin, comprising the following components in parts by weight:

[0006]

[0007] Furthermore, the epoxy resin is one or two of E51 and E44.

[0008] Furthermore, the curing agent is dicyandiamide.

[0009] Furthermore, the accelerator is at least one of organic urea, imidazole and modified imidazole accelerator.

[0010] Furthermore, the thickener is at least one of liquid amines having primary and / or secondary amino groups, wherein the molar ratio of the total amount of active hydrogen of the primary and / or secondary amino groups to the epoxy group of the epoxy resin is 0.05-0.3.

[0011] Furthermore, the filler is a hydrophilic aerogel, the hydrophilic aerogel has a particle size D50≤5 microns, an average pore size≤30 nm, and a hydrophilic surface.

[0012] Furthermore, the diluent is composed of one or more reactive diluents containing at least one epoxy functional group.

[0013] Furthermore, the auxiliary agent is at least one of a coupling agent, a viscosity reducer, a wetting agent, a dispersant, a defoaming agent, a toughening agent, a wetting agent, and an internal release agent.

[0014] The impregnating agent is epoxy resin impregnating agent EP880.

[0015] The thickener includes one or more of alicyclic amines and fatty amines such as ethylenediamine, diethylenetriamine, triethylenetetramine, isophoronediamine, and methylcyclohexanediamine.

[0016] Furthermore, the viscosity of the low-density heat-insulating epoxy resin is 13000-15000 mP·s, the density is 1.05-1.15 g / cm3, and the thermal conductivity is 0.14-0.16.

[0017] According to a second aspect of the present application, the present application provides a method for preparing a low-density thermal insulation epoxy resin, the preparation method comprising the following steps:

[0018] Step 1, weighing 90-110 parts by weight of epoxy resin, adding 2-10 parts by weight of thickener and 1-10 parts by weight of auxiliary agent to obtain a first resin mixture;

[0019] Step 2: Place the first resin mixture in step 1 into a high-speed disperser for thorough mixing.

[0020] Step 3, leaving the mixture in step 2 at a temperature of 30-50° C. for 30-60 minutes;

[0021] Step 4, adding filler to the resin mixture fully dispersed and mixed in step 3 to obtain a second resin mixture;

[0022] Step 5: After the second resin mixture in step 4 is fully mixed with a high-speed disperser, 2-20 parts by weight of a curing agent and 1-8 parts by weight of an accelerator are added to obtain a third resin mixture.

[0023] Step 6, the third resin mixture in step 5 is fully mixed with a high-speed disperser and placed in a curing room for curing;

[0024] Step 7: Place the third resin mixture matured in step 6 on a press for compression molding to obtain a low-density heat-insulating epoxy resin sheet.

[0025] Furthermore, in step 2, the speed of the high-speed disperser is 900-1100 r / min, and the stirring time is 5-10 min;

[0026] In step 5, the speed of the high-speed disperser is 300-400 r / min. After stirring for 5-10 min, the speed of the high-speed dispersant is adjusted to 500-600 r / min, and the stirring time is 10-15 min.

[0027] In step 6, the speed of the high-speed disperser is 500-600 r / min, and the stirring time is 3-10 min;

[0028] In step 6, the aging temperature is 25-45° C. and the aging time is 15-30 hours;

[0029] In step 7, the press temperature is 140-160° C., and the molding time is 3-8 min.

[0030] The invention provides a low-density heat-insulating epoxy resin and a preparation method thereof. The low-density heat-insulating epoxy resin comprises the following components in parts by weight: 90-110 parts of epoxy resin, 2-20 parts of curing agent, 1-8 parts of accelerator, 5-20 parts of diluent, 1-10 parts of auxiliary agent, 2-10 parts of thickener, and 2-5 parts of filler. The thickener is first added to the epoxy resin to increase the viscosity of the epoxy resin, reduce the probability of mixing the resin with the high specific area filler, or reduce the penetration of the resin into the micropores of the aerogel, prevent the filler of the porous structure from being filled with the resin, and then add the filler (aerogel) to effectively reduce the density of the material from 1.2g / cm 3 Reduced to 1.1g / cm 3 Moreover, the low-density thermal insulation epoxy resin does not contain volatile substances during production, and there is no VOC emission in the production process, which is more environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] The above and other purposes, features and advantages of the present invention will become more apparent by describing the embodiments of the present invention in more detail in conjunction with the accompanying drawings. The accompanying drawings are used to provide a further understanding of the embodiments of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings, the same reference numerals generally represent the same components or steps. DETAILED DESCRIPTION

[0032] Below, the exemplary embodiments according to the present invention will be described in detail with reference to the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments of the present invention, and it should be understood that the present invention is not limited to the exemplary embodiments described here.

[0033] Example 1

[0034] 97g of bisphenol A glycidyl ether type liquid epoxy resin E-51, 1g of epoxy resin impregnating agent EP880, 5g of internal release agent epoxy silicone oil BD-1208, and 4.4g of alicyclic amine were placed in a reaction kettle and dispersed and stirred at high speed for 8 minutes to mix evenly; after standing for 30 minutes, 1g of aerogel was added and dispersed and stirred at low speed for 10 minutes, and after the aerogel was completely soaked, the speed was increased and stirred for 15 minutes; finally, 7g of dicyandiamide and 2g of organic urea were added and stirred for 7 minutes, and the composite material was obtained after being sent to a 35°C drying room for aging for 20 hours.

[0035] The prepared composite material was rapidly cured at 150°C for 5 min and then used for press plate testing.

[0036] Example 2

[0037] 100g of bisphenol A glycidyl ether type liquid epoxy resin E-51, 1g of epoxy resin impregnating agent EP880, 5g of internal release agent epoxy silicone oil BD-1208, and 4.4g of diethylenetriamine were placed in a reaction kettle and dispersed and stirred at high speed for 8min to mix evenly; after standing for 30min, 1g of aerogel was added and dispersed and stirred at low speed for 10min, and after the aerogel was completely impregnated, the speed was increased and stirred for 15min; finally, 7g of dicyandiamide and 2g of organic urea were added, stirred for 9min, and sent to a 40°C drying room for aging for 20h to obtain a composite material.

[0038] The prepared composite material was rapidly cured at 150°C for 5 min and then used for press plate testing.

[0039] Example 3

[0040] 100g of bisphenol A glycidyl ether type liquid epoxy resin E-51, 1g of epoxy resin impregnating agent EP880, 6g of internal release agent epoxy silicone oil BD-1208, and 4.4g of alicyclic amine were placed in a reaction kettle and dispersed and stirred at high speed for 9 minutes to mix evenly; after standing for 30 minutes, 1.5g of aerogel was added and dispersed and stirred at low speed for 10 minutes, and after the aerogel was completely soaked, the speed was increased and stirred for 15 minutes; then 7g of dicyandiamide and 2g of organic urea were added, stirred for 7 minutes, and sent to a 40°C drying room for aging for 20 hours to obtain a composite material.

[0041] The prepared composite material was rapidly cured at 150°C for 5 min and then used for press plate testing.

[0042] Example 4

[0043] 97g of bisphenol A glycidyl ether type liquid epoxy resin E-51, 1g of epoxy resin impregnating agent EP880, 5g of diethylenetriamine, and 5g of internal release agent epoxy silicone oil BD-1208 were placed in a reaction kettle and dispersed and stirred at high speed to mix evenly; after standing for 30 minutes, 1.5g of aerogel was added and dispersed and stirred at low speed for 10 minutes, and after the aerogel was completely soaked, the speed was increased and stirred for 15 minutes; then 7g of dicyandiamide, 2g of organic urea, and 1g of imidazole were added, stirred for 7 minutes, and sent to a 40°C drying room for aging for 20 hours to obtain a composite material.

[0044] The prepared composite material was rapidly cured at 150°C for 5 min and then used for press plate testing.

[0045] Example 5

[0046] 110g of bisphenol A glycidyl ether type liquid epoxy resin E-51, 5g of internal release agent epoxy silicone oil BD-1208, 1g of epoxy resin impregnating agent EP880, and 5g of diethylenetriamine were placed in a reaction kettle and dispersed and stirred at high speed to mix evenly; after standing for 30 minutes, 2g of aerogel was added and dispersed and stirred at low speed for 10 minutes, and after the aerogel was completely soaked, the speed was increased and stirred for 15 minutes; then 7g of dicyandiamide and 2g of organic urea were added, stirred for 7 minutes, and sent to a 40°C drying room for aging for 20 hours to obtain a composite material.

[0047] The prepared composite material was rapidly cured at 150°C for 5 min and then used for press plate testing.

[0048] Example 6

[0049] 97g of bisphenol A glycidyl ether type liquid epoxy resin E-51, 6g of internal release agent epoxy silicone oil BD-1208, 0.5g of epoxy resin impregnating agent EP880, and 5g of diethylenetriamine were placed in a reaction kettle and dispersed and stirred at high speed to mix evenly; after standing for 30 minutes, 2.5g of aerogel was added and dispersed and stirred at low speed for 10 minutes, and after the aerogel was completely soaked, the speed was increased and stirred for 15 minutes; then 7g of dicyandiamide and 2g of organic urea were added, stirred for 7 minutes, and sent to a 40°C drying room for aging for 20 hours to obtain a composite material.

[0050] The prepared composite material was rapidly cured at 150°C for 5 min and then used for press plate testing.

[0051] Example 7

[0052] 110g of bisphenol A glycidyl ether type liquid epoxy resin E-51, 5g of internal mold release agent epoxy silicone oil BD-1208, 1g of epoxy resin impregnating agent EP880, and 5g of diethylenetriamine are placed in a reaction kettle and dispersed and stirred at high speed to mix evenly; after standing for 30 minutes, 2.5g of aerogel is added and dispersed and stirred at low speed for 10 minutes, and after the aerogel is completely soaked, the speed is increased and stirred for 15 minutes; then 7g of dicyandiamide and 1.5g of organic urea are added, stirred for 7 minutes, and sent to a 40°C drying room for aging for 20 hours to obtain a composite material.

[0053] The prepared composite material was rapidly cured at 150°C for 5 min and then used for press plate testing.

[0054] Comparative Example 1

[0055] 103g of bisphenol A glycidyl ether type liquid epoxy resin E-51, 5g of internal release agent epoxy silicone oil BD-1208, and 2g of epoxy resin impregnating agent EP880 are dispersed and stirred at high speed to mix evenly; then 30g of glass beads are added and dispersed and stirred at low speed for 10 minutes, and after the glass beads are completely soaked, the speed is increased and stirred for 15 minutes; 7g of dicyandiamide, 2g of organic urea, 1g of imidazole, and 5g of fatty amine are added, stirred for 7 minutes, and sent to a 40°C drying room for curing for 20 hours to obtain a composite material.

[0056] The prepared composite material was rapidly cured at 150°C for 5 min and then used for press plate testing.

[0057] Comparative Example 2

[0058] 100g of bisphenol A glycidyl ether type liquid epoxy resin E-51, 5g of internal release agent epoxy silicone oil BD-1208, and 1g of epoxy resin impregnating agent EP880 were dispersed and stirred at high speed to mix evenly; then 2.5g of aerogel was added and dispersed and stirred at low speed for 10min, and after the aerogel was completely impregnated, the speed was increased and stirred for 15min; 7g of dicyandiamide, 1.5g of organic urea, and 5g of diethylenetriamine were added, stirred for 7min, and sent into a 40°C drying room for curing for 20h to obtain a composite material.

[0059] The prepared composite material was rapidly cured at 150°C for 5 min and then used for press plate testing.

[0060] Comparative Example 3

[0061] 103g of bisphenol A glycidyl ether type liquid epoxy resin E-51, 5g of internal release agent epoxy silicone oil BD-1208, and 1g of epoxy resin impregnating agent EP880 are dispersed and stirred at high speed to mix evenly; 7g of dicyandiamide, 2g of organic urea, 1g of imidazole, and 5g of diethylenetriamine are added, stirred for 7 minutes, and sent to a 40°C drying room for curing for 20 hours to obtain a composite material.

[0062] The prepared composite material was rapidly cured at 150°C for 5 min and then used for press plate testing.

[0063] Table 1 Test data of embodiments and comparative examples

[0064] <![CDATA[Viscosity (a) (mP·s)]]> <![CDATA[Density (g / cm 3 )]]> Thermal conductivity Example 1 14113 1.12 0.16 Example 2 14372 1.12 0.16 Example 3 13899 1.11 0.15 Example 4 14314 1.13 0.15 Example 5 14366 1.10 0.15 Example 6 14657 1.10 0.15 Example 7 14036 1.11 0.15 Comparative Example 1 4421 1.04 0.18 Comparative Example 2 4233 1.15 0.16 Comparative Example 3 -- 1.20 0.20

[0065] Note: (a) is the resin viscosity at 25°C before adding filler.

[0066] As can be seen from Table 1, compared with the comparative example, the viscosity of the epoxy resin composite material prepared in the embodiment is greatly increased by first adding the curing agent and the accelerator to the epoxy resin, compared with the traditional method of first adding the epoxy resin and the filler and then adding the curing agent and the accelerator. The viscosity of the traditional addition method is between 4233-4421mP·s, while the viscosity of the curing agent and the accelerator added first in the embodiment of the present invention is between 13899-14657mP·s. The increase in viscosity reduces the penetration of the resin into the micropores of the aerogel and prevents the filler of the porous structure from being filled with the resin. The addition of the aerogel leads to a decrease in the density of the prepared epoxy resin composite material, and the density increases from 1.2g / cm 3 Reduced to 1.1g / cm 3 Comparative Example 3 has the highest density of 1.2 g / cm2 due to the absence of filler. 3 Glass microspheres are added to Comparative Example 1, and the glass microspheres have the effect of reducing density, so the density of Comparative Example 1 is the lowest. The addition of aerogel reduces the thermal conductivity of the epoxy resin composite material. After adding aerogel, the thermal conductivity of the epoxy resin is reduced from 0.20 to 0.15. The diluent added during the production of the low-density thermal insulation epoxy resin is an active diluent, which does not contain volatile substances. There is no VOC emission in the production process, which is more environmentally friendly.

[0067] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the concept and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A low-density thermal insulation epoxy resin, characterized in that: The composition comprises the following components in parts by weight:

2. A low-density thermal insulation epoxy resin according to claim 1, characterized in that: The epoxy resin is one or two of E51 and E44; The curing agent is dicyandiamide.

3. A low-density thermal insulation epoxy resin according to claim 1, characterized in that: The accelerator is at least one of organic urea, imidazole and modified imidazole accelerator.

4. A low-density thermal insulation epoxy resin according to claim 1, characterized in that: The thickener is at least one of liquid amines having primary and / or secondary amino groups, wherein the molar ratio of the total amount of active hydrogen of the primary and / or secondary amino groups to the epoxy group of the epoxy resin is 0.05-0.

3.

5. A low-density thermal insulation epoxy resin according to claim 1, characterized in that: The filler is a hydrophilic aerogel, the hydrophilic aerogel particle size D50 is ≤5 microns, the average pore size is ≤30nm, and the surface is hydrophilic.

6. A low-density heat-insulating epoxy resin according to claim 5, characterized in that: The diluent is composed of one or more reactive diluents containing at least one epoxy functional group.

7. A low-density heat-insulating epoxy resin according to claim 6, characterized in that: The auxiliary agent is at least one of a coupling agent, a wetting agent, a dispersant, a defoamer, a toughening agent, a wetting agent, and an internal release agent; The impregnating agent is epoxy resin impregnating agent EP880; The thickener includes one or more of modified amines of ethylenediamine, diethylenetriamine, triethylenetetramine, meta-xylylenediamine, isophoronediamine, methylcyclohexanediamine, alicyclic amines and aromatic amines.

8. A low-density thermal insulation epoxy resin according to claim 1, characterized in that: The viscosity of the low-density heat-insulating epoxy resin is 13000-15000mP·s and the density is 1.05-1.15g / cm 3 , the thermal conductivity is 0.14-0.

16.

9. A method for preparing a low-density heat-insulating epoxy resin, characterized in that: The steps include: Step 1, weighing 90-110 parts by weight of epoxy resin, adding 2-10 parts by weight of thickener and 1-10 parts by weight of auxiliary agent to obtain a first resin mixture; Step 2: Place the first resin mixture in step 1 into a high-speed disperser for thorough mixing. Step 3, leaving the mixture in step 2 at a temperature of 30-50° C. for 30-60 minutes; Step 4, adding filler to the resin mixture fully dispersed and mixed in step 3 to obtain a second resin mixture; Step 5: After the second resin mixture in step 4 is fully mixed with a high-speed disperser, 2-20 parts by weight of a curing agent and 1-8 parts by weight of an accelerator are added to obtain a third resin mixture. Step 6, the third resin mixture in step 5 is fully mixed with a high-speed disperser and placed in a curing room for curing; Step 7: Place the third resin mixture matured in step 6 on a press for compression molding to obtain a low-density heat-insulating epoxy resin sheet.

10. The method for preparing a low-density heat-insulating epoxy resin according to claim 9, characterized in that: In step 2, the speed of the high-speed disperser is 900-1100 r / min, and the stirring time is 5-10 min; In step 5, the speed of the high-speed disperser is 300-400 r / min. After stirring for 5-10 min, the speed of the high-speed dispersant is adjusted to 500-600 r / min, and the stirring time is 10-15 min. In step 6, the speed of the high-speed disperser is 500-600 r / min, and the stirring time is 3-10 min; In step 6, the aging temperature is 25-45° C. and the aging time is 15-30 hours; In step 7, the press temperature is 140-160° C., and the molding time is 3-8 min.