Biodegradable master batch for express bag and preparation method of biodegradable master batch
By compounding PLA, PBS, agricultural waste fillers, and ECO materials, and adding CNC as a reinforcing filler, biodegradable masterbatch was prepared, solving the environmental pollution problem caused by traditional express delivery bags and achieving high-performance material substitution and resource utilization.
Patent Information
- Application Number
- CN202410417673.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-08
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional express delivery bags are mainly made of plastic products, which leads to environmental pollution and energy consumption. Furthermore, the lack of an effective waste recycling mechanism causes land pollution and health hazards.
A biodegradable masterbatch was prepared by compounding PLA, PBS, agricultural waste filler, wetting agent and elastomer ECO, and adding CNC as a reinforcing filler, through mixing, melting and extrusion, to improve the mechanical properties and toughness of the material.
The prepared biodegradable masterbatch material has good mechanical properties and toughness, and can effectively replace traditional plastic express delivery bags, reduce environmental pollution, and improve crop utilization.
Smart Images

Figure SMS_1 
Figure HDA0005024131920000011
Abstract
Description
Technical Field
[0001] The invention relates to a biodegradable masterbatch for express bags and a preparation method thereof, and belongs to the technical field of material preparation. Background Art
[0002] Since the mid-20th century, with the rapid development of China's economy and the significant improvement of its scientific and technological level, the types of logistics packaging have been continuously enriched and the forms have been innovated, ushering in a golden age of vigorous development. Among packaging materials, plastic film is widely used in production lines and logistics packaging scenarios of many products such as food, beverages, medicine, and daily necessities due to its advantages such as moisture-proof and anti-oxidation, flexibility and durability, and lightness and transparency. The express delivery industry is one of the fastest-growing industries in my country in recent years. Due to the rise of online shopping and e-commerce, the business volume of the express delivery industry has grown at a high rate of 50% per year in the past five years. At the same time, express delivery companies use a large amount of packaging materials to ensure the safety of goods and meet the conditions of express delivery. Traditional express delivery packaging materials are divided into seven categories: express waybills, plastic woven bags, plastic bags, envelopes, packaging boxes, tapes, and internal buffers. Among them, the consumption of plastic products is astonishing. Taking plastic bags as an example, the average basic quantity used in the past three years is about 7 billion per year, causing great environmental pollution and energy consumption.
[0003] Plastic bags and woven bags are mainly made of materials such as PE and PP. Since my country has not yet established an effective garbage recycling mechanism, most of the discarded plastic bags and woven bags are landfilled or incinerated. Landfilling is very harmful to the land, and incomplete incineration of plastic products will produce toxic and harmful substances such as dioxins, which are extremely harmful to human health. Summary of the invention
[0004] In view of the above problems existing in the prior art, the object of the present invention is to provide a biodegradable masterbatch for express bags and a preparation method thereof.
[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:
[0006] A biodegradable masterbatch for express bags and a preparation method thereof, characterized in that the biodegradable masterbatch is mainly prepared from the following raw materials in parts by weight:
[0007] PLA 15-25 parts;
[0008] PBS 5-10 parts;
[0009] 70-80 parts of agricultural waste filler;
[0010] Wetting agent 0.5-1 part;
[0011] Elastomer 5-10 parts.
[0012] As a preferred embodiment, each portion of the agricultural waste filler is obtained by mixing cellulose (CNC), wild rice leaves, and a filler surface modifier in a weight ratio of 1 to 2:5 to 8:1, wherein CNC is extracted from waste straw, and wild rice leaves are organic flocculent fiber substances obtained by processing waste wild rice leaves.
[0013] As a preferred solution, each portion of the filler surface modifier is a mixture of ethyl cellulose, cyclodextrin, and glycosylglycerol in a weight ratio of (5-10): (7-13): 20.
[0014] As a preferred embodiment, the elastomer is epichlorohydrin elastomer (ECO).
[0015] As a preferred embodiment, the CNC is prepared by the following steps:
[0016] a) washing agricultural waste straw (such as wheat straw), pressing water, drying, alkali soaking, alcohol washing, drying again, crushing and sieving to obtain natural fiber;
[0017] b) reacting the natural fiber obtained in step a at 80-160° C. for 30-200 min to complete liquefaction, adjusting the pH of the liquefied product to 6.5-7.5, adding a filler surface modifier and mixing evenly, crushing, sieving, obtaining CNC, and weighing;
[0018] The amount of the filler surface modifier used is 0.1 to 0.15 times the weight of the natural fiber in step b.
[0019] As a preferred embodiment, the agricultural waste filler is prepared by the following steps:
[0020] a) According to parts by weight: weigh wild rice stem leaves and filler surface modifier, stir them evenly at a temperature of 50 to 60° C. for 30 to 40 minutes to obtain a mixture A;
[0021] b) By weight: weigh CNC and mix the mixture A evenly to obtain an agricultural waste filler.
[0022] As a further preferred embodiment, a method for preparing a biodegradable masterbatch for a courier bag comprises the following steps:
[0023] a) weighing 2 / 3 parts by weight of the agricultural waste filler and mixing it with PLA to prepare a mixture B;
[0024] b) kneading the remaining 1 / 3 of the agricultural waste filler with PBS according to the weight parts to obtain a mixture C;
[0025] c) uniformly mixing the mixture B, the mixture C, the wetting agent and the elastomer, kneading, melting, extruding and pelletizing to obtain a biodegradable masterbatch.
[0026] Compared with the prior art, the present invention has the following significant beneficial effects:
[0027] The present invention uses PLA, PBS, agricultural waste fillers, wetting agents and elastomers in a compounded manner. The raw materials are all degradable materials. The added CNC is used as an ideal reinforcing filler, which has the advantage of improving the mechanical properties of polymer composite materials. This is because when an appropriate amount of CNC is added to the system, CNC can be well dispersed in the matrix. Due to the mechanical permeation effect between the matrix and CNC and the strong interaction between CNC itself, the composite material obtains better mechanical properties, but the two form a rigid interconnected network structure due to hydrogen bonding to resist the stretching process, resulting in effective stress transfer from the flexible matrix to the rigid CNC nanostructures. However, when the CNC content is too high, the self-aggregation between CNCs to form a rigid network hinders the interaction between the molecular interfaces, which will cause the elastic modulus and elongation at break of the composite material to decrease. In the system, ECO can improve the toughness of PLA, thereby improving the strength of the degradable masterbatch, and improving the strength and toughness of the courier bag. This is because ECO contains a small amount of ionizable groups in the main chain of the macromolecule, and the hydrogen bonds formed by the reaction between it and the polymer are the main reason for the toughening effect. Most of the agricultural waste fillers are composed of wild rice leaf waste, which effectively improves the utilization rate of crops. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is the microstructure morphology of the masterbatch; DETAILED DESCRIPTION
[0029] The following is a further detailed and complete description of the technical solution of the present invention in combination with specific embodiments and comparative examples. The materials selected in this application can all be obtained from the market, and the sources and models of some raw materials are shown in Table 1:
[0030] Table 1 Sources and models of some raw materials
[0031]
[0032] Example 1
[0033] A biodegradable masterbatch for express bags and a preparation method thereof, wherein the biodegradable masterbatch is mainly prepared by the following steps:
[0034] S1. Preparing agricultural waste filler, the specific steps include:
[0035] S1-1, weigh 0.5 kg of wild rice stem leaves and 0.1 kg of surface modifier, and stir them evenly at 50° C., wherein the weights of ethyl cellulose, cyclodextrin, and glycosylglycerol in the surface modifier are 0.01 kg, 0.02 kg, and 0.07 kg, respectively;
[0036] S1-2, washing 1 kg of wheat straw, pressing water, drying, alkali soaking, alcohol washing, drying again, crushing and sieving to obtain natural fiber;
[0037] S1-3, reacting the natural fiber obtained in step 1-2 at 100° C. for 60 min to complete liquefaction, adjusting the pH of the liquefied product to 7.0, adding a filler surface modifier, mixing evenly, crushing, and sieving to obtain CNC;
[0038] S1-4, weigh 0.03 kg of CNC and a mixture of S1-1, mix them evenly at 40° C., crush them, and pass them through a 100-mesh sieve to obtain agricultural waste filler;
[0039] S2, weighing 0.42 kg of the natural filler prepared in S1-2 and 0.14 kg of PLA, and kneading them to obtain a mixture B;
[0040] S3, weighing 0.21 kg of the natural filler prepared in S1-2 and 0.6 kg of PBS, and kneading them to obtain a mixture C;
[0041] S4. Mix mixture B, mixture C, 0.004 kg of wetting agent and 0.04 kg of ECO uniformly, and perform mixing, melting, extrusion and pelletizing to obtain a biodegradable masterbatch.
[0042] Example 2
[0043] A biodegradable masterbatch for express bags and a preparation method thereof, wherein the biodegradable masterbatch is mainly prepared by the following steps:
[0044] S1. Preparing agricultural waste filler, the specific steps include:
[0045] S1-1, weigh 0.7 kg of wild rice stem leaves and 0.2 kg of surface modifier, and stir them evenly at 60° C., wherein the weights of ethyl cellulose, cyclodextrin, and glycosylglycerol in the surface modifier are 0.01 kg, 0.02 kg, and 0.07 kg, respectively;
[0046] S1-2, washing 1 kg of wheat straw, pressing water, drying, alkali soaking, alcohol washing, drying again, crushing and sieving to obtain natural fiber;
[0047] S1-3, the natural fiber obtained in step 1-2 is reacted at 110° C. for 50 min to complete liquefaction, the pH of the liquefied product is adjusted to 7.0, a filler surface modifier is added, mixed evenly, crushed, and sieved to obtain CNC;
[0048] S1-4, weigh 0.05 kg of CNC and a mixture of S1-1, mix them evenly at 40° C., crush them, and pass them through a 100-mesh sieve to obtain agricultural waste filler;
[0049] S2, weighing 0.5 kg of the natural filler prepared in S1-2 and 0.16 kg of PLA and kneading them to obtain a mixture B;
[0050] S3, weighing 0.3 kg of the natural filler prepared in S1-2 and 0.7 kg of PBS, and kneading them to obtain a mixture C;
[0051] S4. Mix mixture B, mixture C, 0.004 kg of wetting agent and 0.04 kg of ECO uniformly, and perform mixing, melting, extrusion and pelletizing to obtain a biodegradable masterbatch.
[0052] Example 3
[0053] A biodegradable masterbatch for express bags and a preparation method thereof, wherein the biodegradable masterbatch is mainly prepared by the following steps:
[0054] S1. Preparing agricultural waste filler, the specific steps include:
[0055] S1-1, weigh 1 kg of wild rice stem leaves and 0.2 kg of a surface modifier, and stir them evenly at 50° C., wherein the weights of ethyl cellulose, cyclodextrin, and glycosylglycerol in the surface modifier are 0.02 kg, 0.02 kg, and 0.06 kg, respectively;
[0056] S1-2, washing 2 kg of wheat straw, pressing water, drying, alkali soaking, alcohol washing, drying again, crushing and sieving to obtain natural fiber;
[0057] S1-3, reacting the natural fiber obtained in step 1-2 at 100° C. for 60 min to complete liquefaction, adjusting the pH of the liquefied product to 7.0, adding a filler surface modifier, mixing evenly, crushing, and sieving to obtain CNC;
[0058] S1-4, weigh 0.06 kg of CNC and a mixture of S1-1, mix them evenly at 40° C., crush them, and pass them through a 100-mesh sieve to obtain agricultural waste filler;
[0059] S2, weighing 0.85 kg of the natural filler prepared in S1-2 and 0.26 kg of PLA, and kneading them to obtain a mixture B;
[0060] S3, weighing 0.45 kg of the natural filler prepared in S1-2 and 1.2 kg of PBS, and kneading them to obtain a mixture C;
[0061] S4. Mix mixture B, mixture C, 0.008 kg of wetting agent and 0.08 kg of ECO uniformly, and perform mixing, melting, extrusion and pelletizing to obtain a biodegradable masterbatch.
[0062] Comparative Example 1
[0063] The difference between this comparative example and Example 1 is that an equal amount of PBAT is used instead of PLA, and the other raw materials and amounts are consistent with Example 1. The PBAT used in this comparative example has a purity of Mn-120000 and is purchased from Shanghai Gaoxin Chemical Glass Instrument Co., Ltd. The brand is McLean and the grade is P909229.
[0064] Comparative Example 2
[0065] The difference between this comparative example and Example 1 is that an equal amount of PBAT is used instead of PBS, and the other raw materials and amounts are consistent with those in Example 1.
[0066] Performance Test:
[0067] 1. Microscopic morphology test
[0068] After the biodegradable masterbatch was melt-formed and mechanically tested, samples were taken from the fracture surface and the fracture surface morphology of the composite material was observed using a JSM-5610LV scanning electron microscope. An acceleration voltage of 5 kV was applied and the magnification was adjusted to 300. The microscopic morphology was as follows: Figure 1 shown.
[0069] 2. Mechanical properties test
[0070] After the biodegradable masterbatch was melt-formed, the tensile properties were tested in accordance with GB / T1447-2005. The MTS universal strength tester was used to cut I-type dumbbell-shaped specimens according to the standard. The length was 180 mm, the width of the two ends was 20 mm, the width of the middle parallel section was 10 mm, the thickness of the specimen was 2 mm, the test speed was 10 mm / min, and the tensile properties test results are shown in Table 2.
[0071] Table 2
[0072] Tensile strength / MPa Example 1 62.24 Example 2 60.08 Example 3 58.21 Comparative Example 1 55.24 Comparative Example 2 32.20
[0073] 3. Thermal stability test
[0074] A TG-209F3 thermogravimetric analyzer was selected to detect the thermal stability of the material. The sample size was about 5 mg. The test was carried out under nitrogen atmosphere protection. The flow rate was set to 10 ml / min, and the temperature was increased at a rate of 10 °C / min. The temperature range was 25 °C to 650 °C. The test results are shown in Table 3.
[0075] Table 3
[0076] Thermal stability parameters / ℃ Example 1 301.25 Example 2 299.82 Example 3 305.65 Comparative Example 1 285.67 Comparative Example 2 275.98
Claims
1. A biodegradable masterbatch for express bags and a preparation method thereof, characterized in that: The degradable masterbatch is mainly prepared from the following raw materials in parts by weight: PLA 15-25 parts; PBS 5-10 parts; 70-80 parts of agricultural waste filler; Wetting agent 0.5-1 part; Elastomer 5-10 parts.
2. The degradable masterbatch according to claim 1, characterized in that: Each portion of the agricultural waste filler is obtained by mixing cellulose (CNC), wild rice leaves and filler surface modifier in a weight ratio of 1-2:5-8:1, wherein CNC is extracted from waste straw, and wild rice leaves are organic flocculent fiber materials obtained by processing waste wild rice leaves.
3. The agricultural waste filler according to claim 2, characterized in that: Each portion of the filler surface modifier is prepared by mixing ethyl cellulose, cyclodextrin and glycosylglycerol in a weight ratio of (5-10): (7-13):
20.
4. The degradable masterbatch according to claim 1, characterized in that: The elastomer is epichlorohydrin rubber elastomer (ECO).
5. The degradable masterbatch according to claim 1, characterized in that: The CNC is prepared by the following steps: a) washing agricultural waste straw (such as wheat straw), pressing water, drying, alkali soaking, alcohol washing, drying again, crushing and sieving to obtain natural fiber; b) reacting the natural fiber obtained in step a at 80-160° C. for 30-200 min to complete liquefaction, adjusting the pH of the liquefied product to 6.5-7.5, adding a filler surface modifier and mixing evenly, crushing, sieving, obtaining CNC, and weighing; The amount of the filler surface modifier used is 0.1 to 0.15 times the weight of the natural fiber in step b.
6. The degradable masterbatch according to claim 1, characterized in that: The agricultural waste filler is prepared by the following steps: a) According to parts by weight: weigh wild rice stem leaves and filler surface modifier, stir them evenly at a temperature of 50 to 60° C. for 30 to 40 minutes to obtain a mixture A; b) By weight: weigh CNC and mix the mixture A evenly to obtain an agricultural waste filler.
7. A method for preparing a biodegradable masterbatch for courier bags as claimed in any one of claims 1 to 5, characterized in that: The following steps are involved: a) weighing 2 / 3 parts by weight of the agricultural waste filler and mixing it with PLA to prepare a mixture B; b) kneading the remaining 1 / 3 of the agricultural waste filler with PBS according to the weight parts to obtain a mixture C; c) uniformly mixing the mixture B, the mixture C, the wetting agent and the elastomer, kneading, melting, extruding and pelletizing to obtain a biodegradable masterbatch.