High-performance carbon dioxide-epoxypropane modified copolymer and preparation method thereof
By blending polybutylene succinate segments and silica, combined with isocyanate end-blocking treatment, the problem of insufficient thermal stability and mechanical properties of carbon dioxide-propylene oxide copolymer is solved, and high performance is achieved Thermal stability and barrier properties are improved.
Patent Information
- Application Number
- CN202410997761.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
AI Technical Summary
The thermal stability and mechanical properties of carbon dioxide-propylene oxide copolymers are poor, and are prone to deformation and adhesion at high temperatures. The compatibility of the prior art is difficult to regulate when blending modified materials, resulting in a degradation of performance.
Polybutylene succinate segments are grafted with terminal hydroxyl groups and blended with silica and heat stabilizer using polybutylene succinate by grafting the polybutylene succinate segments with terminal hydroxyl groups as the active site and blending them with silica and thermal stabilizers. The ester-based stability and physical barrier effect of silica form a dense structure to improve thermal stability and mechanical strength while reducing the dezip degradation reaction by isocyanate capping.
The thermal stability, mechanical strength and barrier properties of the carbon dioxide-propylene oxide modified copolymer are significantly improved, the compatibility problems are solved, and the impact toughness and gas and water vapor barrier properties of the material are enhanced.
Smart Images

Figure BDA0004960728730000101 
Figure BDA0004960728730000111 
Figure BDA0004960728730000112
Abstract
Description
Technical Field
[0001] The present application relates to the field of biodegradable materials, and in particular to a high-performance carbon dioxide-propylene oxide modified copolymer and a preparation method thereof. Background Art
[0002] Biodegradable polypropylene carbonate can be obtained by copolymerization of carbon dioxide and propylene oxide. This type of copolymer can not only effectively utilize carbon dioxide resources and reduce the expansion of the greenhouse effect, but also reduce the use of petroleum-based products. It is a kind of environmentally friendly material with great development prospects. In addition, carbon dioxide-propylene oxide copolymers also have good biocompatibility, biodegradability and physical and mechanical properties, and have broad application prospects in the fields of packaging materials, fibers and nonwovens.
[0003] However, since the carbon dioxide-propylene oxide copolymer is an amorphous substance and cannot be crystallized, the molecules are highly flexible and the intermolecular interaction is small, resulting in a low glass transition temperature and poor mechanical properties compared to other biodegradable materials. It is also easy to deform and adhere at higher temperatures. To solve the above problems, the prior art often uses different materials to blend and modify the carbon dioxide-propylene oxide copolymer to obtain a composite material with excellent performance. Among them, polybutylene succinate with excellent mechanical properties and high heat deformation temperature has been blended with carbon dioxide-propylene oxide copolymer to obtain a composite material, thereby improving the performance of the copolymer. However, in the application process, polybutylene succinate, as a semi-crystalline compound, is difficult to control the compatibility with the carbon dioxide-propylene oxide copolymer, which will cause the performance of the obtained blend to decrease. Summary of the invention
[0004] In order to solve the problem of poor thermal stability of carbon dioxide-propylene oxide copolymers, the present application provides a high-performance carbon dioxide-propylene oxide modified copolymer and a preparation method thereof, thereby obtaining a carbon dioxide-propylene oxide modified copolymer with high mechanical strength, good thermal stability and excellent barrier properties.
[0005] In a first aspect, the present application provides a high-performance carbon dioxide-propylene oxide modified copolymer, wherein the high-performance carbon dioxide-propylene oxide modified copolymer comprises the following raw materials in parts by weight: 100 parts of carbon dioxide-propylene oxide graft copolymer; 2-5 parts of silicon dioxide; Heat stabilizer 0.5-1.5 parts; The carbon dioxide-propylene oxide graft copolymer contains polybutylene succinate chain segments.
[0006] Preferably, the heat stabilizer includes one or a combination of maleic anhydride, succinic anhydride, glutaric anhydride, phthalic anhydride, and tetrahydrophthalic anhydride.
[0007] By adopting the above technical solution, in order to reduce the compatibility problems caused by physical blending and improve the thermal stability and other properties of the carbon dioxide-propylene oxide copolymer, a graft modification treatment is performed on it, specifically: The carbon dioxide-propylene oxide graft copolymer is a grafted polybutylene succinate chain segment with the terminal hydroxyl group of the carbon dioxide-propylene oxide copolymer as the active site. On the one hand, the ester group contained in the polybutylene succinate chain segment has stable chemical properties and good thermal stability, and its ester bond structure can remain stable in a wide temperature range, thereby improving the overall thermal stability. On the other hand, the terminal hydroxyl group is reacted as an active site to reduce the "unzipping" degradation reaction caused by the active chemical properties of the terminal hydroxyl group, thereby improving the thermal stability of the carbon dioxide-propylene oxide copolymer. In addition, the copolymerization modification method can solve the problem of poor compatibility that may exist in the physical blending modification process, improve the molecular structure of the carbon dioxide-propylene oxide copolymer, and thus significantly improve the thermal stability and mechanical strength of the material.
[0008] At the same time, by grafting polybutylene succinate chain segments, more crosslinking points can be introduced into the carbon dioxide-propylene oxide copolymer, the interaction between polymer molecules can be enhanced, and a denser structure can be formed. While improving the mechanical strength of the material, the material can also improve its barrier properties to oxygen and water vapor and reduce permeation. In addition, due to its certain crystallization ability, the grafted polybutylene succinate chain segments may separate from the main chain carbon dioxide-propylene oxide copolymer to form a microphase separation structure. This structure can effectively hinder crack propagation, thereby significantly improving the impact strength and toughness of the carbon dioxide-propylene oxide copolymer material.
[0009] The carbon dioxide-propylene oxide graft copolymer obtained at last is blended with silicon dioxide and a heat stabilizer. As an inorganic filler, silicon dioxide can improve the rigidity and hardness of the carbon dioxide-propylene oxide graft copolymer to a certain extent, and increase the wear resistance of the material. In addition, silicon dioxide also has good thermal stability, which can improve the thermal decomposition stability and the use temperature range of the copolymer, and improve the stability in a high temperature environment. The physical barrier layer formed can also effectively reduce the permeability of small molecules such as oxygen and water vapor, and improve the gas barrier and water vapor barrier properties of the material. The carbon dioxide-propylene oxide modified copolymer obtained at last has good thermal stability, as well as excellent mechanical properties and barrier properties.
[0010] Preferably, the raw materials of the carbon dioxide-propylene oxide graft copolymer include a carbon dioxide-propylene oxide copolymer, a polybutylene succinate prepolymer and a polybutylene succinate monomer in a mass ratio of 1: (0.05-0.15): (0.1-0.2); the polybutylene succinate monomer is succinic acid and butanediol in a molar ratio of 1: (1.1-1.2).
[0011] By adopting the above technical scheme, in the preparation process of the carbon dioxide-propylene oxide graft copolymer, the polybutylene succinate prepolymer is used as a bridge to connect the carbon dioxide-propylene oxide copolymer and use it as an active site to further polymerize the polybutylene succinate chain segment on it, thereby improving the thermal stability and other properties of the material.
[0012] Preferably, the carbon dioxide-propylene oxide copolymer is end-capped with isocyanate.
[0013] Preferably, the isocyanate includes one or a combination of toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate.
[0014] By adopting the above technical scheme, in order to further improve the grafting rate of the polybutylene succinate chain segment on the carbon dioxide-propylene oxide copolymer, the carbon dioxide-propylene oxide copolymer is firstly subjected to isocyanate end-capping treatment, the isocyanate group in the isocyanate can undergo addition reaction with the terminal hydroxyl group in the carbon dioxide-propylene oxide copolymer, and the isocyanate group with strong reaction activity is introduced into the molecular chain of the carbon dioxide-propylene oxide copolymer, which can attract the hydroxyl group in the polybutylene succinate prepolymer to react, thereby further realizing the grafting modification of the polybutylene succinate chain segment.
[0015] At the same time, after being capped with isocyanate, the terminal hydroxyl content in the carbon dioxide-propylene oxide copolymer can be greatly reduced, thereby reducing the "unzipping" degradation reaction at the end, thereby improving the high-temperature stability of the copolymer and improving the thermal stability of the material.
[0016] Preferably, the carbon dioxide-propylene oxide graft copolymer is prepared according to the following method: Preparation of carbon dioxide-propylene oxide copolymer: under nitrogen atmosphere, add the dehydrated propylene oxide and catalyst 1 to a reactor, fill with carbon dioxide gas to a pressure of 3-5 MPa, adjust the reaction temperature to 50-80°C, stir for 8-12 hours, and obtain carbon dioxide-propylene oxide copolymer; End-capping treatment of the carbon dioxide-propylene oxide copolymer: adding isocyanate to the obtained carbon dioxide-propylene oxide copolymer for plasticization and end-capping, wherein the reaction temperature is adjusted to 110-120° C., reacting for 10-30 minutes, washing, filtering and drying to obtain the carbon dioxide-propylene oxide copolymer after isocyanate end-capping treatment; Preparation of polybutylene succinate prepolymer: under nitrogen atmosphere, succinic acid, butanediol and catalyst 2 are added to solvent 1, and reacted at 140-160° C. for 1-2 hours to obtain polybutylene succinate prepolymer, wherein the molar ratio of succinic acid to butanediol is 1:(1.1-1.2); Graft modification of carbon dioxide-propylene oxide copolymer: Under a nitrogen atmosphere, polybutylene succinate prepolymer and catalyst 3 are added to the carbon dioxide-propylene oxide copolymer that has been end-capped with isocyanate, the reaction temperature is adjusted to 120-150°C, and after stirring and reacting for 2-3 hours, polybutylene succinate monomer and catalyst 2 are added, and the reaction is continued for 4-6 hours. Finally, the carbon dioxide-propylene oxide graft copolymer is obtained by washing, filtering and drying.
[0017] Preferably, the catalyst 1 is a bimetallic catalyst, which is one or a combination of two of Zn-Co based bimetallic cyanide and Fe / Zn bimetallic cyanide; the catalyst 2 includes one or a combination of several of stannous chloride, stannous octoate, dibutyltin dilaurate, and tetraisopropyl titanate; the catalyst 3 includes one or a combination of several of triethylamine, dimethylethanolamine, N,N'-dimethylformamide, and triethanolamine.
[0018] Preferably, the mass ratio of the carbon dioxide-propylene oxide copolymer to the isocyanate is 1:(0.01-0.02).
[0019] Preferably, the solvent 1 comprises one or a combination of toluene, xylene, decahydronaphthalene and tetrahydrofuran.
[0020] By adopting the above technical scheme, the carbon dioxide-propylene oxide copolymer is first synthesized, and the isocyanate group in the isocyanate is further used to react with the terminal hydroxyl group to form a stable chemical bond to control the chain growth, which is conducive to the grafting of the polybutylene succinate chain segment. Secondly, under the action of catalyst 2, succinic acid and butanediol are esterified and polymerized to obtain a polybutylene succinate prepolymer, and the low-molecular-weight prepolymer can be better dispersed in the carbon dioxide-propylene oxide copolymer and reacted and connected with the active groups on the carbon dioxide-propylene oxide copolymer after the isocyanate end-capping treatment, and can better induce succinic acid and butanediol to extend the chain on the prepolymer, so that the polybutylene succinate chain segment is smoothly grafted on the carbon dioxide-propylene oxide copolymer.
[0021] Preferably, the silica is siloxane-acrylate copolymer modified silica; the raw materials of the siloxane-acrylate copolymer modified silica include silica, siloxane monomer and glycidyl methacrylate in a mass ratio of 1: (0.05-0.1): (2-4).
[0022] Preferably, the siloxane monomer includes one or a combination of vinyl triethoxysilane, methacryloxypropyl triethoxysilane, γ-methacryloxypropylene trimethoxysilane, and vinyl trimethoxysilane.
[0023] By adopting the above technical solution, the blending of carbon dioxide-propylene oxide grafted copolymer and silica can utilize the properties of silica itself, and the thermal stability and mechanical strength of the final material can be improved to a certain extent. However, the dispersibility of silica in the polymer is limited to a certain extent, and the inability to disperse evenly also has a certain impact on the performance of the obtained material. Therefore, in this application, siloxane-acrylate copolymer is used to modify silica.
[0024] Specifically, the modified silica has better compatibility and dispersibility with the carbon dioxide-propylene oxide graft copolymer, and can be evenly distributed in the copolymer during the mixing process, giving full play to the performance advantages of silica. In addition, the active groups contained in the acrylate copolymer formed by glycidyl methacrylate can react with the hydroxyl or carboxyl groups contained in the carbon dioxide-propylene oxide graft copolymer, thereby forming a tight network structure, which can enhance the mechanical properties of the material, and the tight network structure combined with the physical barrier effect of silica can further improve the barrier properties of the material. The siloxane structure has a higher bond energy and better stability, and after combining with the carbon dioxide-propylene oxide graft copolymer, it can increase the free volume between molecules, which helps to relieve thermal stress and enhance the thermal stability of the material.
[0025] Preferably, the siloxane-acrylate copolymer modified silica is prepared according to the following method: dispersing silica in solvent 2, adding siloxane monomer, stirring at 80-100° C. for 1-2 hours to obtain siloxane-grafted silica; adding glycidyl methacrylate to solvent 3, stirring and mixing, adding siloxane-grafted silica and initiator, adjusting the reaction temperature to 60-90° C., reacting for 5-6 hours, washing, drying and grinding to obtain siloxane-acrylate copolymer modified silica.
[0026] Preferably, solvent 2 is one of ethanol aqueous solution, isopropanol aqueous solution and acetone aqueous solution.
[0027] Preferably, solvent 3 is one of acetone and ethyl acetate.
[0028] Preferably, the initiator includes one or a combination of ammonium persulfate, potassium persulfate, and azobisisobutyronitrile; the added amount of the initiator is 0.5-1% of the mass of glycidyl methacrylate.
[0029] By adopting the above technical scheme, the surface of silica contains a large number of hydroxyl groups, which can undergo condensation reaction with the hydrolyzed siloxane monomer to form a stable silicon-oxygen bond. The siloxane chain segment is first grafted to the surface of silica, and then the active group in the siloxane chain segment serves as the active initiation point for acrylate polymerization. Under the action of the initiator, glycidyl methacrylate undergoes copolymerization reaction to form a siloxane-acrylate copolymer on the surface of silica, thereby improving the compatibility and dispersibility of silica in the copolymer and improving the performance of the composite material.
[0030] In a second aspect, the present application also provides a method for preparing a high-performance carbon dioxide-propylene oxide modified copolymer, comprising the following process steps: S1. Weigh the carbon dioxide - propylene oxide graft copolymer, silica and heat stabilizer in parts by mass and mix them in a high-mixer to obtain a premix; S2. The premix is dried and then plasticized in an internal mixer to obtain a high-performance carbon dioxide-propylene oxide modified copolymer, wherein the internal mixer temperature is 120 to 140°C.
[0031] In summary, this application has the following beneficial effects: 1. The high-performance carbon dioxide-propylene oxide modified copolymer of the present application contains a carbon dioxide-propylene oxide graft copolymer. Specifically, the carbon dioxide-propylene oxide graft copolymer uses the terminal hydroxyl groups of the carbon dioxide-propylene oxide copolymer as active sites, and grafts polybutylene succinate chain segments, which can solve the problem of poor compatibility that may exist in the physical blending modification process, and improve the molecular structure of the carbon dioxide-propylene oxide copolymer, thereby significantly improving the thermal stability and mechanical strength of the material. In addition, the ester structure in the polybutylene succinate is stable, which improves the good thermal stability, and the terminal hydroxyl groups of the carbon dioxide-propylene oxide copolymer are connected by reaction, which can also reduce the "unzipping" degradation reaction caused by the active chemical properties of the terminal hydroxyl groups. After grafting, the molecular chain contains more crosslinking points, which can form a more compact structure, and can improve the material's barrier properties to oxygen and water vapor while improving the mechanical strength of the material.
[0032] 2. The high-performance carbon dioxide-propylene oxide modified copolymer of the present application also contains silicon dioxide. The silicon dioxide is modified by the siloxane-acrylate copolymer, which can significantly improve the compatibility and dispersibility of silicon dioxide in the carbon dioxide-propylene oxide graft copolymer. The active groups contained in the acrylate copolymer formed by glycidyl methacrylate can react with the hydroxyl or carboxyl groups contained in the carbon dioxide-propylene oxide graft copolymer to form a tight network structure, which can enhance the mechanical properties of the material. The tight network structure combined with the physical barrier effect of silicon dioxide can further improve the barrier properties of the material, and the introduction of silicon-oxygen bonds can further improve the thermal stability. DETAILED DESCRIPTION
[0033] Preparation Example of Carbon Dioxide-Propylene Oxide Graft Copolymer Preparation Example 1-1, a carbon dioxide-propylene oxide graft copolymer, is prepared according to the following method: Preparation of carbon dioxide-propylene oxide copolymer: under nitrogen atmosphere, add the dehydrated propylene oxide and Zn-Co based double metal cyanide catalyst into a reactor, fill with carbon dioxide gas to a pressure of 4 MPa, adjust the reaction temperature to 70°C, stir for 12 hours, and obtain carbon dioxide-propylene oxide copolymer; The Zn-Co based double metal cyanide catalyst is prepared according to the following method: a zinc chloride solution with a mass fraction of 50% is added dropwise to a rapidly stirred potassium hexacyanocobaltate solution, a white precipitate is generated, the precipitate is re-slurried with a tert-butyl alcohol aqueous solution, and the precipitate is separated again. The steps are repeated until there are no free potassium ions in the solution, and the Zn-Co based double metal cyanide catalyst is finally obtained by centrifugation, separation and drying.
[0034] End-capping treatment of the carbon dioxide-propylene oxide copolymer: 20 g of diphenylmethane diisocyanate was added to 1 kg of the obtained carbon dioxide-propylene oxide copolymer for plasticization and end-capping, wherein the reaction temperature was adjusted to 120° C., and after reacting for 20 minutes, the carbon dioxide-propylene oxide copolymer was washed, filtered and dried to obtain an isocyanate-end-capped carbon dioxide-propylene oxide copolymer; Preparation of polybutylene succinate prepolymer: In a nitrogen atmosphere, 250 g of a mixture of succinic acid and butanediol and 2.5 g of stannous chloride were added to 500 ml of toluene solution, and the mixture was reacted at 150° C. for 2 h to obtain a polybutylene succinate prepolymer, wherein the molar ratio of succinic acid to butanediol was 1:1.1; Carbon dioxide-propylene oxide copolymer graft modification: In a nitrogen atmosphere, 0.1 kg of polybutylene succinate prepolymer and 1 g of N,N'-dimethylformamide were added to 1 kg of carbon dioxide-propylene oxide copolymer that had been treated with isocyanate end capping, and the reaction temperature was adjusted to 140°C. After stirring for 2 hours, 0.15 kg of polybutylene succinate monomer and 1.5 g of stannous chloride were added, and the reaction was continued for 5 hours. Finally, the carbon dioxide-propylene oxide graft copolymer was obtained after washing, filtering and drying. The polybutylene succinate monomer is succinic acid and butanediol with a molar ratio of 1:1.2.
[0035] Preparation Example 1-2, a carbon dioxide-propylene oxide graft copolymer, differs from Preparation Example 1-1 only in that, during the graft modification of the carbon dioxide-propylene oxide copolymer, the amount of polybutylene succinate prepolymer added is 0.05 kg and the amount of polybutylene succinate monomer added is 0.1 kg.
[0036] Preparation Example 1-3, a carbon dioxide-propylene oxide graft copolymer, differs from Preparation Example 1-1 only in that, during the graft modification of the carbon dioxide-propylene oxide copolymer, the amount of polybutylene succinate prepolymer added is 0.15 kg and the amount of polybutylene succinate monomer added is 0.2 kg.
[0037] Preparation Example 1-4, a carbon dioxide-propylene oxide graft copolymer, is different from Preparation Example 1-1 only in that, during the graft modification of the carbon dioxide-propylene oxide copolymer, the amount of polybutylene succinate prepolymer added is 0.02 kg.
[0038] Preparation Example 1-5, a carbon dioxide-propylene oxide graft copolymer, is different from Preparation Example 1-1 only in that, during the graft modification of the carbon dioxide-propylene oxide copolymer, the amount of polybutylene succinate prepolymer added is 0.2 kg.
[0039] Preparation Example 1-6, a carbon dioxide-propylene oxide graft copolymer, is different from Preparation Example 1-1 only in that, during the graft modification of the carbon dioxide-propylene oxide copolymer, the amount of polybutylene succinate monomer added is 0.05 kg.
[0040] Preparation Example 1-7, a carbon dioxide-propylene oxide graft copolymer, is different from Preparation Example 1-1 only in that, during the graft modification of the carbon dioxide-propylene oxide copolymer, the amount of polybutylene succinate monomer added is 0.25 kg.
[0041] Preparation Example 1-8 is a carbon dioxide-propylene oxide graft copolymer, which is different from Preparation Example 1-1 only in that the carbon dioxide-propylene oxide copolymer is not end-capped with diphenylmethane diisocyanate.
[0042] Preparation Example 1-9, a carbon dioxide-propylene oxide graft copolymer, is different from Preparation Example 1-1 only in that no polybutylene succinate prepolymer is added during the graft modification of the carbon dioxide-propylene oxide copolymer.
[0043] Preparation Example of Siloxane-Acrylate Copolymer Modified Silica Preparation Example 2-1, a siloxane-acrylate copolymer modified silica, prepared according to the following method: Take 10g of silica (average particle size of 1μm) and disperse it in 250ml of 75% ethanol aqueous solution, add 0.8g of methacryloyloxypropyltriethoxysilane, and stir at 80°C for 2h to obtain siloxane-grafted silica; add 30g of glycidyl methacrylate to acetone, stir and mix, then add to obtain siloxane-grafted silica and 0.3g of azobisisobutyronitrile, adjust the reaction temperature to 80°C, react for 6h, wash, dry and grind to obtain siloxane-acrylate copolymer modified silica.
[0044] Preparation Example 2-2, a siloxane-acrylate copolymer modified silica, is different from Preparation Example 2-1 only in that the added amount of methacryloxypropyltriethoxysilane is 0.5 g; the added amount of glycidyl methacrylate is 20 g.
[0045] Preparation Example 2-3, a siloxane-acrylate copolymer modified silica, is different from Preparation Example 2-1 only in that the added amount of methacryloxypropyltriethoxysilane is 1 g; the added amount of glycidyl methacrylate is 40 g.
[0046] Preparation Example 2-4, a siloxane-acrylate copolymer modified silica, is different from Preparation Example 2-1 only in that the added amount of glycidyl methacrylate is 10 g.
[0047] Preparation Example 2-5, a siloxane-acrylate copolymer modified silica, is different from Preparation Example 2-1 only in that the added amount of glycidyl methacrylate is 50 g.
[0048] Preparation Example 2-6, a siloxane-acrylate copolymer modified silica, was prepared according to the following method: 10 g of silica (average particle size of 1 μm) was dispersed in 250 ml of 75% ethanol aqueous solution, 0.8 g of methacryloxypropyltriethoxysilane was added, and stirred at 80°C for 2 hours to obtain siloxane-grafted silica, and then washed, dried and ground to obtain siloxane-acrylate copolymer modified silica. Example
[0049] Example 1, a high-performance carbon dioxide-propylene oxide modified copolymer, prepared according to the following method: S1. Weigh 1kg of carbon dioxide - propylene oxide graft copolymer, 32g of silicon dioxide (average particle size of 1 μm) and 10g of glutaric anhydride, and mix them in a high-speed stirrer to obtain a premix; S2. The premix is dried and then plasticized in an internal mixer to obtain a high-performance carbon dioxide-propylene oxide modified copolymer, wherein the internal mixer temperature is 130°C.
[0050] Example 2, a high-performance carbon dioxide-propylene oxide modified copolymer, is different from Example 1 only in that the added amount of silicon dioxide is 20 g and the added amount of glutaric anhydride is 5 g.
[0051] Example 3, a high-performance carbon dioxide-propylene oxide modified copolymer, is different from Example 1 only in that the added amount of silicon dioxide is 50 g and the added amount of glutaric anhydride is 15 g.
[0052] Example 4, a high-performance carbon dioxide-propylene oxide modified copolymer, is different from Example 1 only in that the carbon dioxide-propylene oxide graft copolymer prepared in Preparation Example 1-1 is replaced by an equal amount of the carbon dioxide-propylene oxide graft copolymer prepared in Preparation Example 1-2.
[0053] Example 5, a high-performance carbon dioxide-propylene oxide modified copolymer, is different from Example 1 only in that the carbon dioxide-propylene oxide graft copolymer prepared in Preparation Example 1-1 is replaced by an equal amount of the carbon dioxide-propylene oxide graft copolymer prepared in Preparation Example 1-3.
[0054] Example 6, a high-performance carbon dioxide-propylene oxide modified copolymer, is different from Example 1 only in that the carbon dioxide-propylene oxide graft copolymer prepared in Preparation Example 1-1 is replaced by an equal amount of the carbon dioxide-propylene oxide graft copolymer prepared in Preparation Example 1-4.
[0055] Example 7, a high-performance carbon dioxide-propylene oxide modified copolymer, is different from Example 1 only in that the carbon dioxide-propylene oxide graft copolymer prepared in Preparation Example 1-1 is replaced by an equal amount of the carbon dioxide-propylene oxide graft copolymer prepared in Preparation Example 1-5.
[0056] Example 8, a high-performance carbon dioxide-propylene oxide modified copolymer, is different from Example 1 only in that the carbon dioxide-propylene oxide graft copolymer prepared in Preparation Example 1-1 is replaced by an equal amount of the carbon dioxide-propylene oxide graft copolymer prepared in Preparation Example 1-6.
[0057] Example 9, a high-performance carbon dioxide-propylene oxide modified copolymer, is different from Example 1 only in that the carbon dioxide-propylene oxide graft copolymer prepared in Preparation Example 1-1 is replaced by an equal amount of the carbon dioxide-propylene oxide graft copolymer prepared in Preparation Example 1-7.
[0058] Example 10, a high-performance carbon dioxide-propylene oxide modified copolymer, is different from Example 1 only in that the carbon dioxide-propylene oxide graft copolymer prepared in Preparation Example 1-1 is replaced by an equal amount of the carbon dioxide-propylene oxide graft copolymer prepared in Preparation Example 1-8.
[0059] Example 11, a high-performance carbon dioxide-propylene oxide modified copolymer, is different from Example 1 only in that the carbon dioxide-propylene oxide graft copolymer prepared in Preparation Example 1-1 is replaced by an equal amount of the carbon dioxide-propylene oxide graft copolymer prepared in Preparation Example 1-9.
[0060] Example 12, a high-performance carbon dioxide-propylene oxide modified copolymer, is different from Example 1 only in that silica is replaced by an equal amount of siloxane-acrylate copolymer modified silica prepared in Preparation Example 2-1.
[0061] Example 13, a high-performance carbon dioxide-propylene oxide modified copolymer, differs from Example 12 only in that the siloxane-acrylate copolymer modified silica prepared in Preparation Example 2-1 is replaced by an equal amount of the siloxane-acrylate copolymer modified silica prepared in Preparation Example 2-2.
[0062] Example 14, a high-performance carbon dioxide-propylene oxide modified copolymer, differs from Example 12 only in that an equal amount of the siloxane-acrylate copolymer modified silica prepared in Preparation Example 2-3 is used to replace the siloxane-acrylate copolymer modified silica prepared in Preparation Example 2-1.
[0063] Example 15, a high-performance carbon dioxide-propylene oxide modified copolymer, differs from Example 12 only in that an equal amount of the siloxane-acrylate copolymer modified silica prepared in Preparation Example 2-4 is used to replace the siloxane-acrylate copolymer modified silica prepared in Preparation Example 2-1.
[0064] Example 16, a high-performance carbon dioxide-propylene oxide modified copolymer, differs from Example 12 only in that an equal amount of the siloxane-acrylate copolymer modified silica prepared in Preparation Example 2-5 is used to replace the siloxane-acrylate copolymer modified silica prepared in Preparation Example 2-1.
[0065] Example 17, a high-performance carbon dioxide-propylene oxide modified copolymer, differs from Example 12 only in that the siloxane-acrylate copolymer modified silica prepared in Preparation Example 2-1 is replaced with an equal amount of the siloxane-acrylate copolymer modified silica prepared in Preparation Example 2-6.
[0066] Comparative Example Comparative Example 1 is a high-performance carbon dioxide-propylene oxide modified copolymer, which is different from Example 1 only in that the amount of silicon dioxide added is 10 g.
[0067] Comparative Example 2 is a high-performance carbon dioxide-propylene oxide modified copolymer, which is different from Example 1 only in that the amount of silicon dioxide added is 70 g.
[0068] Comparative Example 3 is a high-performance carbon dioxide-propylene oxide modified copolymer, which is different from Example 1 only in that silicon dioxide is not added.
[0069] Comparative Example 4, a high-performance carbon dioxide-propylene oxide modified copolymer, was prepared according to the following method: S1. Weigh 0.8 kg of the carbon dioxide-propylene oxide copolymer prepared in Preparation Example 1-1, 0.2 kg of polybutylene succinate (model FZ91PM), 32 g of silicon dioxide (average particle size of 1 μm) and 10 g of glutaric anhydride, and mix them in a high-speed stirrer to obtain a premix; S2. The premix is dried and then plasticized in an internal mixer to obtain a high-performance carbon dioxide-propylene oxide modified copolymer, wherein the internal mixer temperature is 130°C.
[0070] Comparative Example 5, a high-performance carbon dioxide-propylene oxide modified copolymer, was prepared according to the following method: S1. Weigh 1 kg of the carbon dioxide - propylene oxide copolymer prepared in Preparation Example 1-1, 32 g of silicon dioxide (average particle size of 1 μm) and 10 g of glutaric anhydride, and mix them in a high stirrer to obtain a premix; S2. The premix is dried and then plasticized in an internal mixer to obtain a high-performance carbon dioxide-propylene oxide modified copolymer, wherein the internal mixer temperature is 130°C.
[0071] Performance testing 1. Mechanical strength performance test: (1) Tensile strength test: According to the relevant records in GB / T 1040-2008 "Determination of tensile properties of plastics", the high-performance carbon dioxide-propylene oxide modified copolymers obtained in the examples and comparative examples were subjected to a tensile strength test.
[0072] (2) Impact strength test: According to the relevant records in GB / T 1843-2008 “Determination of Izod impact strength of plastics”, the high-performance carbon dioxide-propylene oxide modified copolymers obtained in the examples and comparative examples were subjected to a tensile strength test.
[0073] 2. Thermal stability test: The samples obtained in the embodiments and comparative examples were placed in an oven at 120° C. and left to stand for three days. The tensile strength of the materials was tested after three days.
[0074] The above test results are shown in Table 1.
[0075] 3. Barrier performance test: According to GB / T 1037-2021 “Determination of water vapor permeability of plastic films and sheets - Cup weight gain and weight loss method” and ISO 2556:2001 “Plastic films and sheets - Determination of air permeability under atmospheric pressure - Pressure measurement method”, the water vapor and oxygen barrier properties of the embodiments and comparative examples were tested respectively.
[0076] The barrier performance test results are shown in Table 2.
[0077] Table 1 Mechanical properties and thermal stability test results Table 2 Barrier performance test results According to Table 1 and Table 2, in combination with Example 1, Example 2 to Example 5, it can be seen that the impact strength, oxygen and water vapor transmission rate, and tensile strength before and after high temperature treatment of Example 2 to Example 5 are not significantly different from those of Example 1, indicating that the mechanical properties, thermal stability, and barrier properties of Example 2 to Example 5 are not significantly different from those of Example 1. The reason may be that the difference between Example 2 to Example 5 and Example 1 is only that the raw material ratio and the raw material ratio of the carbon dioxide-propylene oxide graft copolymer used are changed within the required range, resulting in no significant difference in the performance changes of the final obtained materials.
[0078] Combining Example 1 and Example 6 to Example 11, it can be seen that the impact strength and tensile strength before and after high temperature treatment of Example 6 to Example 11 are lower than those of Example 1, and the oxygen and water vapor permeability are higher, indicating that the mechanical properties, thermal stability and barrier properties of Example 6 to Example 11 are lower than those of Example 1. The reason may be that the difference between Example 6 to Example 11 and Example 1 is that the carbon dioxide-propylene oxide graft copolymer used has an out-of-range adjustment of the raw material ratio during the preparation process. Specifically, Example 6, Example 7 and Example 11 and Example 8 and Example 9 respectively adjust the addition amount of polybutylene succinate prepolymer and the addition amount of polybutylene succinate monomer. Reducing the addition amount will lead to a decrease in the content of the obtained polybutylene succinate segment and a decrease in the improvement effect on the material, while increasing the addition amount will introduce too many crosslinking points, and the rigidity of the material is too large, which will lead to a decrease in mechanical properties. In Example 10, the carbon dioxide-propylene oxide copolymer was not end-capped, resulting in a decrease in the active centers on the copolymer molecular chain. In addition, due to the lack of end-capping treatment, the content of terminal hydroxyl groups increased, which would lead to a decrease in the thermal stability of the material.
[0079] Combining Example 1, Example 12, and Example 13 to Example 17, it can be seen that the impact strength of Example 12 and the tensile strength before and after high temperature treatment are increased compared with Example 1, and the oxygen and water vapor permeability are decreased, indicating that the mechanical properties, thermal stability and barrier properties of Example 12 are enhanced compared with Example 1. The reason may be that the silicon dioxide added in Example 12 is modified by the siloxane-acrylate copolymer, which can improve the compatibility and dispersibility of silicon dioxide in the system, and the introduction of siloxane and the cross-linking reaction between acrylate and graft copolymer improve the thermal stability and mechanical properties of the system to a certain extent. In Examples 13 and 14, the amount of modified silicone-acrylate copolymer-modified silica added during the preparation process was adjusted within the required range, so the obtained material properties had no significant change compared to Example 12, while in Examples 15 to 17, the amount of glycidyl methacrylate added was changed outside the required range. A reduction in the amount of addition will result in the formation of copolymer molecular segments, affecting the cross-linking reaction between silica and the carbon dioxide-propylene oxide grafted copolymer, thereby resulting in a decrease in performance. If the amount of addition is too much, physical entanglement and chemical cross-linking will form between the formed acrylate copolymers, affecting the dispersibility of silica in the system.
[0080] In combination with Example 1 and Comparative Examples 1 to 3, it can be seen that the mechanical strength of Comparative Examples 1 to 3 is significantly reduced, and the thermal stability and barrier properties are reduced. The reason may be that the difference between Comparative Examples 1 to 3 and Example 1 is only that the amount of silicon dioxide added is adjusted out of range. If the amount of silicon dioxide added is too small, the rigidity and hardness of the material will be reduced, the thermal stability will also be reduced, the physical barrier effect will be reduced, and the barrier properties will also be reduced; too much addition will lead to a decrease in the dispersibility of silicon dioxide, which is easy to agglomerate, and too much rigidity will lead to a significant decrease in toughness and a decrease in impact strength.
[0081] Combining Example 1, Comparative Example 4 and Comparative Example 5, it can be seen that the various properties of Comparative Example 4 and Comparative Example 5 are significantly reduced compared with those of Example 1. The reason may be that the polybutylene succinate in Comparative Example 4 is modified by mixing with a carbon dioxide-propylene oxide copolymer through physical blending, and the compatibility of the two is poor, which leads to a decrease in performance, while there is no modification effect of the polybutylene succinate chain segment in Comparative Example 5, resulting in a significant decrease in the thermal stability and barrier properties of the material.
[0082] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A high-performance carbon dioxide-propylene oxide modified copolymer, characterized in that: The high-performance carbon dioxide-propylene oxide modified copolymer comprises the following raw materials in parts by weight: 100 parts of carbon dioxide-propylene oxide graft copolymer; 2-5 parts of silicon dioxide; Heat stabilizer 0.5-1.5 parts; The carbon dioxide-propylene oxide graft copolymer contains polybutylene succinate chain segments.
2. The high-performance carbon dioxide-propylene oxide modified copolymer according to claim 1, characterized in that: The raw materials of the carbon dioxide-propylene oxide graft copolymer include a carbon dioxide-propylene oxide copolymer, a polybutylene succinate prepolymer and a polybutylene succinate monomer in a mass ratio of 1: (0.05-0.15): (0.1-0.2); the polybutylene succinate monomer is succinic acid and butanediol in a molar ratio of 1: (1.1-1.2).
3. The high performance carbon dioxide-propylene oxide modified copolymer according to claim 2, characterized in that: The carbon dioxide-propylene oxide copolymer is end-capped with isocyanate.
4. The high-performance carbon dioxide-propylene oxide modified copolymer according to claim 3, characterized in that: The isocyanate includes one or a combination of toluene diisocyanate, diphenylmethane diisocyanate, and isophorone diisocyanate.
5. The high-performance carbon dioxide-propylene oxide modified copolymer according to claim 3, characterized in that: The carbon dioxide-propylene oxide graft copolymer is prepared according to the following method: Preparation of carbon dioxide-propylene oxide copolymer: under nitrogen atmosphere, add the dehydrated propylene oxide and catalyst 1 to a reactor, fill with carbon dioxide gas to a pressure of 3-5 MPa, adjust the reaction temperature to 50-80°C, stir for 8-12 hours, and obtain carbon dioxide-propylene oxide copolymer; End-capping treatment of the carbon dioxide-propylene oxide copolymer: adding isocyanate to the obtained carbon dioxide-propylene oxide copolymer for plasticization and end-capping, wherein the reaction temperature is adjusted to 110-120° C., reacting for 10-30 minutes, washing, filtering and drying to obtain the carbon dioxide-propylene oxide copolymer after isocyanate end-capping treatment; Preparation of polybutylene succinate prepolymer: under nitrogen atmosphere, succinic acid, butanediol and catalyst 2 are added to solvent 1, and reacted at 140-160° C. for 1-2 hours to obtain polybutylene succinate prepolymer, wherein the molar ratio of succinic acid to butanediol is 1:(1.1-1.2); Graft modification of carbon dioxide-propylene oxide copolymer: Under a nitrogen atmosphere, polybutylene succinate prepolymer and catalyst 3 are added to the carbon dioxide-propylene oxide copolymer that has been end-capped with isocyanate, the reaction temperature is adjusted to 120-150°C, and after stirring and reacting for 2-3 hours, polybutylene succinate monomer and catalyst 2 are added, and the reaction is continued for 4-6 hours. Finally, the carbon dioxide-propylene oxide graft copolymer is obtained by washing, filtering and drying.
6. The high-performance carbon dioxide-propylene oxide modified copolymer according to claim 5, characterized in that: The catalyst 1 is a bimetallic catalyst, which is one or a combination of two of Zn-Co based bimetallic cyanide and Fe / Zn bimetallic cyanide; the catalyst 2 includes one or a combination of several of stannous chloride, stannous octoate, dibutyltin dilaurate, and tetraisopropyl titanate; the catalyst 3 includes one or a combination of several of triethylamine, dimethylethanolamine, N,N'-dimethylformamide, and triethanolamine.
7. The high performance carbon dioxide-propylene oxide modified copolymer according to claim 1, characterized in that: The silicon dioxide is silicon dioxide modified by a siloxane-acrylate copolymer; the raw materials of the silicon dioxide modified by a siloxane-acrylate copolymer include silicon dioxide, a siloxane monomer and glycidyl methacrylate in a mass ratio of 1: (0.05-0.1): (2-4).
8. The high-performance carbon dioxide-propylene oxide modified copolymer according to claim 1, characterized in that: The siloxane-acrylate copolymer modified silica is prepared according to the following method: dispersing silica in solvent 2, adding siloxane monomer, stirring at 80-100° C. for 1-2 hours to obtain siloxane-grafted silica; adding glycidyl methacrylate to solvent 3, stirring and mixing, adding siloxane-grafted silica and initiator, adjusting the reaction temperature to 60-90° C., reacting for 5-6 hours, washing, drying and grinding to obtain siloxane-acrylate copolymer modified silica.
9. The high-performance carbon dioxide-propylene oxide modified copolymer according to claim 1, characterized in that: The heat stabilizer includes one or a combination of maleic anhydride, succinic anhydride, glutaric anhydride, phthalic anhydride and tetrahydrophthalic anhydride.
10. A method for preparing a high-performance carbon dioxide-propylene oxide modified copolymer according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: S1. Weigh the carbon dioxide - propylene oxide graft copolymer, silica and thermal stabilizer in parts by mass and mix them in a high-mixer to obtain a premix; S2. The premix is dried and then plasticized in an internal mixer to obtain a high-performance carbon dioxide-propylene oxide modified copolymer, wherein the internal mixer temperature is 120 to 140°C.