PCR (Polymerase Chain Reaction) material suitable for interior decoration

By adding large and small molecule chain extenders and modified glass fibers to PCR-PC materials, the odor and performance problems of PCR materials in the automotive interior field are solved, and the mechanical properties and degradation performance of high-end cars are improved, reducing the number of cars Environmental pollution.

CN118909416APending Publication Date: 2024-11-08ANHUI JIANGHUAI AUTOMOBILE GRP CORP LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411089662.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The application of existing PCR materials in the automotive interior field is limited by the problems of large odor and poor performance. In particular, PCR-PC and its alloyed materials are difficult to meet the mechanical properties and emanation requirements of high-end cars, resulting in their application range being affected. limit.

Method used

Reaction of active groups is carried out by adding macromolecular chain extenders and small molecule chain extenders to PCR-PC materials to improve the overall molecular weight, and treatment of glass fibers with weak acids to passivate metal ions, combining modified glass fibers and anti-oxygen to form PC/ABS material suitable for interior use.

Benefits of technology

It improves the mechanical properties and degradation properties of the materials, reduces odor emissions, meets the mechanical properties and appearance requirements of high-end cars, and reduces environmental pollution and resource waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a PCR (Polymerase Chain Reaction) material suitable for interior decoration. The PCR material comprises the following components in parts by weight: 30-70 parts of PCR-PC (Polycarbonate) resin; 10 to 45 parts of ABS resin; 2-20 parts of a toughening agent; 2-5 parts of a chain extender 1; 0.3 to 1.2 parts of a chain extender 2; 10-30 parts of modified glass fiber; 0.2 to 0.6 part of an antioxidant; and 0.2 to 0.5 part of a lubricant. The macromolecular chain extender 1 is added, so that the overall molecular weight of PCR-PC is increased through the reaction of active groups, and the degradation condition of a PCR material is improved; by adding the micromolecular chain extender 2, micromolecular substances generated by degradation can be cross-linked, and the situation that the micromolecular substances are separated out as molecules generating odor and the odor of the material is reduced is avoided. Meanwhile, the glass fibers are treated by weak acid, so that metal ions in the glass fibers can be passivated, and the degradation effect on PC substances is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of materials, and in particular to a PCR material suitable for interior decoration. Background Art

[0002] As a major automobile producer and consumer, China ranks first in the world in automobile production and consumption every year. Post-consumer recycled (PCR) plastics have become one of the important directions to reduce plastic environmental pollution and help the automotive industry move towards "carbon neutrality". The discarded plastics are collected from the recycling stream and then sorted, cleaned and granulated by the mechanical recycling system to produce new plastic particles. The new plastic particles have the same structure as the plastics before recycling, but the overall performance will be reduced. At the same time, due to some of its own shortcomings (such as strong odor and inferior performance to petroleum-based new materials), its application in the automotive industry, especially in the field of automotive interiors, is limited. How to use PCR materials in automotive interior materials with huge consumption has become a common problem faced by automotive interior material manufacturers and vehicle manufacturers.

[0003] In recent years, the consumption of polycarbonate in my country has shown a rapid growth. The environmental and energy problems caused by post-consumer recycled (PCR) polycarbonate, including bucket materials, optical media, scrapped automobile lights and other components, and its effective recycling have not attracted enough attention in the relevant domestic industries. At present, a large number of PCR materials are only recycled and processed as low-end waste plastics, with low technical content, resulting in unstable product quality. PC and PC / ABS modified materials have good physical and mechanical properties and processing properties, and are widely used in automotive interior parts, such as pillars, door panels, central channels, dashboards, etc. in mid-to-high-end cars. PC / ABS materials modified by blending PCR materials are difficult to meet the emission requirements of automotive materials due to their poor odor and VOC. At present, PCR-PC and its alloyed materials can basically only meet the general mechanical properties and appearance requirements of injection molding, and the emission problem of the materials has not been well solved, resulting in the failure of PCR-PC and its alloyed materials to expand their application in the field of automotive interior materials. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a PCR material suitable for interior decoration, wherein the addition of a macromolecular chain extender 1 increases the overall molecular weight of PCR-PC through the reaction of active groups, thereby improving the degradation of the PCR material; the addition of a small molecule chain extender 2 can cross-link the small molecules that have been degraded, thereby preventing these small molecules from being precipitated as molecules that produce odors, thereby reducing the odor of the material. At the same time, weak acid treatment of glass fibers can passivate metal ions in the glass fibers, thereby reducing the degradation effect on PC substances.

[0005] The technical problem to be solved by the present invention is achieved through the following technical solutions:

[0006] A PCR material suitable for interior decoration includes the following components in parts by weight: 30-70 parts of PCR-PC resin; 10-40 parts of ABS resin; 2-20 parts of toughening agent; 2-5 parts of chain extender 1; 0.3-1.2 parts of chain extender 2; 10-30 parts of modified glass fiber; 0.2-0.6 parts of antioxidant; and 0.2-0.5 parts of lubricant.

[0007] Preferably, the above technical solution includes the following components in parts by weight: 30-45 parts of PCR-PC resin; 18-23 parts of ABS resin; 11-15 parts of toughening agent; 2-3 parts of chain extender 1; 0.3-0.6 parts of chain extender 2; 24-30 parts of modified glass fiber; 0.2-0.4 parts of antioxidant; and 0.4-0.5 parts of lubricant.

[0008] Preferably, in the above technical solution, the PCR-PC resin is a copolymer with a melt index of 10-35 g / 10 min at 300° C. / 1.2 kg; the polymerization method of the ABS is bulk polymerization, and the butadiene particle size is 800-1500 μm.

[0009] Preferably, in the above technical solution, the toughening agent is MBS core-shell copolymer or ABS high-rubber powder, and the butadiene particle size of the ABS high-rubber powder is 500-700nm.

[0010] Preferably, in the above technical solution, the chain extender 1 is a random copolymer formed by glycidyl methacrylate and at least two of styrene, acrylonitrile and methyl methacrylate; the weight average molecular weight (Mw) of the chain extender 1 is 6500-80000, and the epoxy equivalent of the chain extender 1 is 200-600 g / mol.

[0011] Preferably, in the above technical solution, the chain extender 2 is a mixture of 2,2'-bis(2-oxazoline), aliphatic glycidyl ether epoxy resin, and polyphenol glycidyl ether epoxy resin, and the molar ratio of the three is (40-60):(10-30):(20-40).

[0012] Preferably, in the above technical solution, the modified glass fiber is at least one of chopped glass fiber and short glass fiber.

[0013] Preferably, in the above technical solution, the modification method comprises the following steps:

[0014] (1) soaking the glass fiber in an acidic solution for 3 to 5 hours, the acid solution temperature being 20 to 30° C.; wherein the acid solution is at least one of acetic acid or citric acid; and the concentration of the acid solution is 2 to 8%;

[0015] (2) Pour off the acid solution and rinse with deionized water until the pH is neutral;

[0016] (3) Soak in 1% to 5% hydrogen peroxide for 1 to 2 hours;

[0017] (4) Filter, wash with deionized water until neutral, and dry to a moisture content of less than 0.15%.

[0018] Preferably, in the above technical solution, the antioxidant is a compound of a hindered phenol antioxidant and a phosphate antioxidant, and the weight ratio of the two is (0.4-2):(2-0.4).

[0019] Preferably, in the above technical scheme, the hindered phenol antioxidant comprises one or more of the following: β-(3-methyl-5-tert-butyl-4-hydroxyphenyl) propionate octadecyl alcohol, tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol methyl ester, 4,4'-thiobis(6-tert-butyl-3-methylphenol); the phosphate antioxidant comprises one or more of the following: 4,4-butylenebis-(3-methyl-6-tert-butylphenyl)-tetrakis(tridecyl) diphosphite, (2,4-di-tert-butyl)phenyl phosphite, at least one of di(2,4-di-tert-butyl)pentaerythritol phosphate, and poly(dipropylene glycol)phenyl phosphite.

[0020] Preferably, in the above technical solution, the lubricant is one or more combinations of stearic acid amide, silicone oil, PE wax, OPE wax, and montan wax.

[0021] A method for preparing a PCR material suitable for interior decoration comprises the following steps:

[0022] (1) Weigh PCR-PC, ABS resin, compatible toughening agent, chain extender, antioxidant, and lubricant according to weight;

[0023] (2) stirring the various raw materials in step (1) uniformly;

[0024] (3) using a high-speed mixer as the stirring device in step (2) and mixing for 3 to 5 minutes for later use;

[0025] (4) The premix obtained in step (3) is fed into a twin-screw extruder through a main feed port, and modified glass fiber is added from a side feed port. After melting, extrusion, water cooling, air drying, and pelletizing, a heat-resistant and low-odor PCR material is obtained.

[0026] Preferably, in the above technical solution, the length-to-diameter ratio (L / D) of the twin-screw extruder is 30 to 40, and a side feeding device is provided.

[0027] Preferably, in the above technical scheme, the temperature of step (4) is 100-250°C, and the screw speed is 250-400rpm. More preferably, the twin-screw extruder is divided into 8 temperature control zones from the feeding port to the outlet, and the specific temperature of each temperature control zone is 100-120°C, 240-250°C, 240-250°C, 240-250°C, 240-250°C, 240-250°C, 240-250°C, 245-250°C, and the screw speed is 280-350rpm.

[0028] The above technical solution of the present invention has the following beneficial effects:

[0029] 1. The addition of macromolecular chain extender 1 increases the overall molecular weight of PCR-PC and improves the degradation of PCR materials through the reaction of active groups.

[0030] 2. The addition of small molecule chain extender 2 can cross-link the small molecules produced by degradation in PCR-PC to prevent the emission of small molecules that have a negative impact on odor;

[0031] 3. Treating the glass fiber with weak acid can passivate the metal ions in the glass fiber and reduce the degradation effect of the glass fiber on the PC material;

[0032] 4. PCR-PC has a wide range of sources. After recycling and reuse, it can avoid environmental pollution, reduce resource waste and carbon emissions. DETAILED DESCRIPTION

[0033] Various exemplary embodiments of the present invention will now be described in detail. It should be noted that the relative arrangement of components and steps, numerical expressions and numerical values ​​set forth in these embodiments do not limit the scope of the present invention unless otherwise specifically stated.

[0034] The PCR-PC used in the following embodiments is a commercially available product, PC 201-10 resin is a product of Trinseo, and ABS is a product of Liaoning Huajin Chemical. The toughening agent is a product of LG of South Korea; the chain extender 1 is SAG-008 of Shanghai Jiayrong; the chain extender 2, antioxidant, and lubricant are commercially available products.

[0035] In addition, the experimental methods used in the following examples are all conventional methods unless otherwise specified, the materials and reagents used are all commercially available unless otherwise specified, and the equipment used in the experiments are all well known to those skilled in the art unless otherwise specified.

[0036] According to the formula in Table 1, the raw materials of Examples 1 to 4 and Comparative Examples 1 to 4 were prepared respectively, and the preparation was carried out according to the above steps. The specific temperatures of each temperature control zone of the twin-screw extruder were 100°C, 240°C, 250°C, 250°C, 250°C, 245°C, 245°C, and 255°C, and the screw speed was 350rpm. The extruded material strips were cooled in a water tank and then pelletized.

[0037] Table 1 Examples and Comparative Examples

[0038]

[0039] The products of the above embodiments and comparative examples were dried in a blast oven at 80°C for 4 hours and then injection molded into standard specimens using a plastic injection molding machine. The injection molded specimens were placed at a relative humidity of 50% and 23°C for at least 24 hours before performance testing.

[0040] Physical performance test conditions: Product performance test methods are as follows:

[0041] The tensile strength of the material is tested based on GB / T 1040.2 standard, the Charpy impact strength of the material is tested based on GB / T 1043.1 standard, the flexural strength and flexural modulus of the material are tested based on GB / T 9341 standard, the odor grade of the material is tested based on PV3900 standard, and the TVOC of the material is tested based on VDA277.

[0042] Table 2 Performance tests of Examples 1 to 4 and Comparative Examples 1 to 4

[0043]

[0044] Note: The lower the odor level, the less odor there is.

[0045] From the above examples and comparative examples, adding chain extender and using modified glass fiber, the mechanical properties, TVOC and odor of Examples 1-2 are significantly better than those of Comparative Examples 1-2; the mechanical properties of Examples 3-5 are slightly better than those of Comparative Examples 3-5 of non-PCR-PC, and the odor and TVOC are significantly better than those of Comparative Examples 3-5. It shows that the mechanical properties of PC / ABS with added chain extender 1, chain extender 2 and modified glass fiber reach the level of new materials, and the TVOC and odor are better.

[0046] Although the present invention has been disclosed as above by the embodiments, it is not intended to limit the present invention. Any person skilled in the art may make various choices and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention is limited by the claims and their equivalents.

Claims

1. A PCR material suitable for interior decoration, It is characterized in that The invention comprises the following components in parts by weight: 30-70 parts of PCR-PC resin; 10-40 parts of ABS resin; 2-20 parts of toughening agent; 12-5 parts of chain extender; 0.3-1.2 parts of chain extender 2; 10-30 parts of modified glass fiber; 0.2-0.6 parts of antioxidant; and 0.2-0.5 parts of lubricant.

2. The PCR material suitable for interior decoration according to claim 1, It is characterized in that The invention comprises the following components in parts by weight: 30-45 parts of PCR-PC resin, 18-23 parts of ABS resin, 11-15 parts of toughening agent, 2-3 parts of chain extender 1, 0.3-0.6 parts of chain extender 2, 24-30 parts of modified glass fiber, 0.2-0.4 parts of antioxidant and 0.4-0.5 parts of lubricant.

3. The PCR material suitable for interior decoration according to claim 1, It is characterized in that The PCR-PC resin is a copolymer with a melt index of 10-35 g / 10 min at 300° C. / 1.2 kg; the polymerization method of the ABS is bulk polymerization, and the butadiene particle size is 800-1500 μm.

4. The PCR material suitable for interior decoration according to claim 1, It is characterized in that The toughening agent is MBS core-shell copolymer or ABS high-rubber powder, and the butadiene particle size of the ABS high-rubber powder is 500-700nm.

5. The PCR material suitable for interior decoration according to claim 1, It is characterized in that The chain extender 1 is a random copolymer formed by glycidyl methacrylate and at least two of styrene, acrylonitrile and methyl methacrylate; the chain extender 2 is a mixture of 2,2'-bis(2-oxazoline), aliphatic glycidyl ether epoxy resin and polyphenol glycidyl ether epoxy resin, and the molar ratio of the three is (40-60):(10-30):(20-40).

6. The PCR material suitable for interior decoration according to claim 1, It is characterized in that The modified glass fiber is at least one of chopped glass fiber and short glass fiber; the modification method comprises the following steps: (1) soaking the glass fiber in an acidic solution for 3 to 5 hours, with the acid solution temperature being 20 to 30° C.; wherein the acid solution is at least one of acetic acid or citric acid; (2) Pour off the acid solution and rinse with deionized water until the pH is neutral; (3) Soak in 1% to 5% hydrogen peroxide for 1 to 2 hours; (4) Filter, wash with deionized water until neutral, and dry to a moisture content of less than 0.15%.

7. The PCR material suitable for interior decoration according to claim 1, It is characterized in that The antioxidant is a compound of a hindered phenol antioxidant and a phosphate antioxidant, and the weight ratio of the two is (0.4-2): (2-0.4).

8. The PCR material suitable for interior decoration according to claim 1, It is characterized in that The lubricant is one or more combinations of stearic acid amides, silicone oil, PE wax, OPE wax, and montan wax.

9. The method for preparing the PCR material suitable for interior decoration according to any one of claims 1 to 8, It is characterized in that The following steps are involved: (1) Weigh PCR-PC, ABS resin, compatible toughening agent, chain extender, antioxidant, and lubricant according to weight; (2) stirring the various raw materials in step (1) uniformly; (3) using a high-speed mixer as the stirring device in step (2) and mixing for 3 to 5 minutes for later use; (4) The premix obtained in step (3) is fed into a twin-screw extruder through a main feed port, and modified glass fiber is added from a side feed port. After melting, extrusion, water cooling, air drying, and pelletizing, a heat-resistant and low-odor PCR material is obtained.

10. The method for preparing the PCR material suitable for interior decoration according to claim 9, It is characterized in that The twin-screw extruder is divided into 8 temperature control zones from the feeding port to the outlet. The specific temperature of each temperature control zone is 100-120℃, 240-250℃, 240-250℃, 240-250℃, 240-250℃, 240-250℃, 240-250℃, 245-250℃, and the screw speed is 280-350rpm.