PC composite material and preparation method and application thereof

By using PCR-PC as a matrix in PC composite materials and adding carbon fibers, toughening agents and chain extenders, the problems of degradation in existing materials and high cost are solved, and high performance and low cost PC composite materials are achieved. Suitable for the manufacturing of electronic and electrical components.

CN118909417APending Publication Date: 2024-11-08DONGGUAN HONOUR E P +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411164399.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The performance of existing PC composite materials has deteriorated in recycling, insufficient antistatic and toughness, and the cost of adding antistatic agents is high, which pollutes the environment and lacks solutions that both low-cost and high-performance.

Method used

Post Consumer Recycling (PCR-PC) is used as the matrix, and carbon fiber, toughener and chain extender are added for collaborative modification to improve antistatic and impact performance, while reducing production costs.

Benefits of technology

It effectively improves the antistatic, impact resistance, mechanical properties and hydrothermal resistance of PC composite materials, reduces carbon emissions and production costs, and makes it suitable for the manufacturing of electronic and electrical components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005007410720000021
    Figure BDA0005007410720000021
  • Figure BDA0005007410720000081
    Figure BDA0005007410720000081
  • Figure BDA0005007410720000082
    Figure BDA0005007410720000082
Patent Text Reader

Abstract

The invention provides a PC composite material and a preparation method and application thereof.The PC composite material comprises specific parts of PCR-PC, carbon fibers, a flexibilizer, a chain extender and a lubricant, the PCR-PC is selected as a matrix, and the specific parts of carbon fibers, the specific parts of flexibilizer and the specific parts of chain extender are added for synergistic modification, so that the PC composite material is obtained. According to the present invention, the carbon emission can be effectively reduced, the production cost of the PC composite material can be reduced, and the antistatic property, the impact resistance, the tensile strength and the hydrothermal aging resistance of the obtained PC composite material can be effectively improved so as to make the PC composite material suitable for preparing electronic and electrical components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite materials, and specifically relates to a PC composite material and a preparation method and application thereof. Background Art

[0002] Post-consumer recycled plastics (PCR) refer to waste plastics generated after use, mainly from components, packaging and other materials of end products. These materials have fulfilled their value in the product circulation chain, but cannot return to the initial end of the product chain. Therefore, they can be turned into valuable industrial production raw materials through physical or chemical recycling. The use of PCR can effectively reduce carbon emissions and is crucial to green and low-carbon development.

[0003] Common PCR materials include PCR-PE, PCR-PP, PCR-ABS, PCR-PC, PCR-PET, PCR-PA, etc.; since it has been heat-processed once and used in various environments, PCR will inevitably have performance degradation after recycling and granulation; especially for PCR-PC, the surface resistivity of conventional PC resin is generally 10 13 ~10 14 The notched impact strength is generally only 65-75 kJ / m 2 , the antistatic properties and toughness are very poor. It is conceivable that the antistatic properties and toughness of PCR-PC are even worse.

[0004] Therefore, in order to improve the antistatic property of PC resin, it is generally modified by adding antistatic agent or conductive carbon black on the market. For example, CN109423023A discloses a halogen-free flame-retardant PC antistatic material and its product; the halogen-free flame-retardant PC antistatic material includes components: PC resin, acetylene carbon black and flame retardant; the product is a product produced after the halogen-free flame-retardant PC antistatic material is formed; the halogen-free flame-retardant PC antistatic material provided by the invention can still have excellent flame retardant properties after adding carbon black by adding compounded flame retardant.

[0005] However, most of the PC composite materials provided in the prior art including the above invention still use ordinary PC resin as the matrix and add antistatic agents for modification. Not only can the waste plastics not be effectively recycled, but also the antistatic agents added are generally expensive and added in large amounts, which not only pollutes the environment but also leads to higher overall costs. In addition, the notched impact strength of the prepared PC material is still low and the toughness still needs to be improved.

[0006] Therefore, in view of the above technical problems, it is urgent to develop a PC composite material with excellent impact resistance, excellent antistatic properties and low cost. Summary of the invention

[0007] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a PC composite material and a preparation method and application thereof. By selecting PCR-PC as a matrix and adding carbon fiber, a toughening agent and a chain extender for synergistic modification, the antistatic and impact resistance of the obtained PC composite material can be effectively improved. At the same time, the carbon emissions can be effectively reduced, and the production cost of the PC composite material can be reduced, making it more suitable for the preparation of electronic and electrical components such as mobile phones and smart watches.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a PC composite material, wherein the PC composite material comprises the following components in parts by weight:

[0010]

[0011] The PC composite material provided by the present invention comprises specific portions of PCR-PC, carbon fiber, toughening agent, chain extender and lubricant; on the one hand, by adopting PCR-PC as a matrix, waste plastics are fully utilized, carbon emissions can be effectively reduced, and the production cost of the PC composite material can be reduced; on the other hand, the PCR-PC is synergistically modified by adding specific portions of carbon fiber, specific portions of toughening agent and specific portions of chain extender, which not only further reduces the preparation cost of the obtained PC composite material, but also effectively improves the antistatic property, impact resistance, mechanical property and water and heat resistance of the obtained PC composite material, making it more suitable for preparing electronic and electrical components such as mobile phones and smart watches.

[0012] Wherein, the content of the PCR-PC can be 60 parts by weight, 61 parts by weight, 62 parts by weight, 63 parts by weight, 64 parts by weight, 65 parts by weight, 66 parts by weight, 67 parts by weight, 68 parts by weight, 69 parts by weight or 70 parts by weight, etc.

[0013] The content of the carbon fiber may be 10 parts by weight, 12 parts by weight, 14 parts by weight, 16 parts by weight, 18 parts by weight, 20 parts by weight, 22 parts by weight, 24 parts by weight, 25 parts by weight, etc.

[0014] The content of the toughening agent can be 1 part by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight, 5 parts by weight, 6 parts by weight, 7 parts by weight or 8 parts by weight, etc.

[0015] The content of the chain extender can be 0.2 parts by weight, 0.3 parts by weight, 0.4 parts by weight, 0.5 parts by weight, 0.6 parts by weight, 0.7 parts by weight or 0.8 parts by weight, etc.

[0016] The content of the lubricant may be 0.1 parts by weight, 0.2 parts by weight, 0.3 parts by weight, 0.4 parts by weight, 0.5 parts by weight, etc.

[0017] Preferably, the melt index of the PCR-PC is 20 to 35 g / 10 min, for example, 20 g / 10 min, 22 g / 10 min, 24 g / 10 min, 26 g / 10 min, 28 g / 10 min, 30 g / 10 min, 32 g / 10 min, 34 g / 10 min or 35 g / 10 min, the test temperature is 300° C., and the load is 1.2 kg.

[0018] Preferably, the carbon fiber is chopped carbon fiber.

[0019] Preferably, the length of the chopped carbon fiber is 4-8 mm, for example, 4 mm, 4.5 mm, 5 mm, 5.5 mm, 6 mm, 6.5 mm, 7 mm, 7.5 mm or 8 mm.

[0020] Preferably, the toughening agent includes any one or a combination of at least two of acrylonitrile-butadiene-styrene copolymer (ABS), methyl methacrylate-butadiene-styrene terpolymer (MBS), methyl methacrylate-acrylate-silicone terpolymer or maleic anhydride grafted polyolefin elastomer (POE-g-MAH graft), and is further preferably a combination of methyl methacrylate-acrylate-silicone terpolymer and maleic anhydride grafted polyolefin elastomer.

[0021] Preferably, the chain extender comprises a styrene-glycidyl methacrylate copolymer.

[0022] Preferably, the lubricant comprises pentaerythritol stearate (PETS) and / or ethylene bis stearamide (EBS).

[0023] Preferably, the PC composite material further comprises any one of PC resin, antioxidant or masterbatch or a combination of at least two thereof.

[0024] Preferably, the content of PC resin in the PC composite material is ≤30 parts by weight, for example, 30 parts by weight, 28 parts by weight, 26 parts by weight, 25 parts by weight, 24 parts by weight, 23 parts by weight, 20 parts by weight, 15 parts by weight, 10 parts by weight or 5 parts by weight.

[0025] Preferably, the melt index of the PC resin is 8 to 17 g / 10 min, for example, 8 g / 10 min, 9 g / 10 min, 10 g / 10 min, 11 g / 10 min, 12 g / 10 min, 13 g / 10 min, 14 g / 10 min, 15 g / 10 min, 16 g / 10 min or 17 g / 10 min, the test temperature is 300 ° C, and the load is 1.2 kg.

[0026] Preferably, the content of the antioxidant in the PC composite material is 0.1 to 0.5 parts by weight, for example, 0.1 parts by weight, 0.2 parts by weight, 0.3 parts by weight, 0.4 parts by weight or 0.5 parts by weight.

[0027] Preferably, the antioxidant comprises a hindered phenol antioxidant and / or a phosphite antioxidant, and more preferably a combination of a hindered phenol antioxidant and a phosphite antioxidant.

[0028] Preferably, the content of the masterbatch in the PC composite material is 0.5 to 1.5 parts by weight, for example, 0.5 parts by weight, 0.7 parts by weight, 0.9 parts by weight, 1 part by weight, 1.1 parts by weight, 1.3 parts by weight or 1.5 parts by weight.

[0029] Preferably, the masterbatch comprises a black masterbatch.

[0030] Preferably, the black masterbatch comprises a PC carrier and carbon black.

[0031] In a second aspect, the present invention provides a method for preparing the PC composite material as described in the first aspect, the preparation method comprising: mixing PCR-PC, carbon fiber, toughening agent, chain extender, lubricant, optionally PC resin, optionally antioxidant and optionally masterbatch, and obtaining the PC composite material by extrusion, cooling, granulation and drying.

[0032] Preferably, the preparation method comprises the following steps:

[0033] (1) drying PCR-PC, carbon fiber, toughening agent, chain extender, lubricant, optionally PC resin, optionally antioxidant and optionally masterbatch to obtain a dry material;

[0034] (2) mixing all dry materials except the dry carbon fiber to obtain a mixed material;

[0035] (3) The mixed material is added into a twin-screw extruder, and dry carbon fiber is added from a side feed port, and the PC composite material is obtained through extrusion, cooling, granulation and drying.

[0036] Preferably, the drying temperature in step (1) is 80-100°C, for example, 80°C, 85°C, 90°C, 95°C or 100°C.

[0037] Preferably, the drying time in step (1) is 1 to 2 hours, for example, 1 hour, 1.2 hours, 1.4 hours, 1.6 hours, 1.8 hours or 2 hours.

[0038] Preferably, the mixing time in step (2) is 6 to 10 min, for example, 6 min, 6.5 min, 7 min, 7.5 min, 8 min, 8.5 min, 9 min, 9.5 min or 10 min.

[0039] Preferably, the mixing in step (2) is carried out at a rotation speed of 600-800 rpm (e.g., 600 rpm, 620 rpm, 640 rpm, 660 rpm, 680 rpm, 700 rpm, 720 rpm, 740 rpm, 760 rpm, 780 rpm or 800 rpm, etc.).

[0040] Preferably, the temperature of the twin-screw extruder in step (3) is 180-255°C, for example, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C or 255°C.

[0041] Preferably, the feeding speed of the twin-screw extruder in step (3) is 12 to 24 rpm, for example, 12 rpm, 14 rpm, 16 rpm, 18 rpm, 20 rpm, 22 rpm or 24 rpm.

[0042] Preferably, the main engine speed of the twin-screw extruder in step (3) is 220-600 rpm, for example, 220 rpm, 240 rpm, 260 rpm, 280 rpm, 300 rpm, 350 rpm, 400 rpm, 450 rpm, 500 rpm, 550 rpm or 600 rpm, etc.

[0043] In a third aspect, the present invention provides an application of the PC composite material as described in the first aspect in an electronic product.

[0044] Compared with the prior art, the present invention has the following beneficial effects:

[0045] (1) The PC composite material provided by the present invention comprises specific portions of PCR-PC, carbon fiber, toughening agent, chain extender and lubricant. By selecting PCR-PC as a matrix and adding specific portions of carbon fiber, specific portions of toughening agent and specific portions of chain extender for synergistic modification, not only can carbon emissions be effectively reduced and the production cost of the PC composite material be reduced, but also the antistatic performance, impact resistance, tensile strength, bending strength and hydrothermal resistance of the obtained PC composite material can be effectively improved, making it suitable for use in the preparation of electronic and electrical components;

[0046] (2) The PC composite material provided by the present invention has a tensile strength of 95-132 MPa, a flexural strength of 127-183 MPa, and a notched impact strength of 8.6-18.2 kJ / m 2 , the surface resistivity at room temperature is 10 7 ~10 10 Ω / m 2 , the surface resistivity after 7 days in a water bath at 70°C is 10 7 ~10 10 Ω / m 2 , with excellent antistatic performance, impact resistance, tensile performance and water and heat aging resistance;

[0047] Moreover, by further optimizing the toughening agent, the PC composite material provided by the present invention can have a tensile strength of up to 107-132 MPa, a flexural strength of up to 147-183 MPa, and a notched impact strength of up to 12.9-18.2 kJ / m 2 , the surface resistivity at room temperature is 10 7 ~10 10 Ω / m 2 , the surface resistivity after 7 days in a water bath at 70°C is 10 7 ~10 10 Ω / m 2 , with the best antistatic properties, impact resistance, tensile properties and water and heat aging resistance. DETAILED DESCRIPTION

[0048] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0049] Some of the raw material information involved in the following specific implementation is as follows:

[0050] (1) PCR-PC: melt index is 25 g / 10 min (300°C / 1.2 kg), purchased from Hunan Jiupeng New Materials Co., Ltd., brand name HNPC20WW;

[0051] (2) PC resin: melt index is 9 g / 10 min (300°C / 1.2 kg), purchased from Luxi Chemical Group Co., Ltd., brand name LXTY1609T-11;

[0052] (3) Chopped carbon fiber: about 6 mm in length, purchased from Japan Polyma Industry Co., Ltd., brand CFUW-MCC-6;

[0053] (4) Conductive carbon black: purchased from Shanghai Guangzhu New Materials Co., Ltd., brand name LITON 25WB;

[0054] (5) Chopped glass fiber: purchased from Taishan Glass Fiber Co., Ltd., brand ECS13-3.0-T442;

[0055] (6) Methyl methacrylate-acrylate-silicone terpolymer: purchased from Mitsubishi Chemical Corporation, brand name S2001;

[0056] (7) POE-g-MAH grafted compound: purchased from DuPont, USA, brand number N216;

[0057] (8) Styrene-methacrylate glycidyl copolymer: purchased from Jiayirong Polymer (Shanghai) Co., Ltd., brand name ECO-1120;

[0058] (9) Antioxidant 1076: hindered phenol antioxidant, commonly available in the market;

[0059] (10) Antioxidant 168: a phosphite antioxidant, commonly available in the market;

[0060] (11) PETS: purchased from Lonza Group, USA, brand number F538;

[0061] (12) EBS: purchased from Kao, Japan;

[0062] (13) Black masterbatch: purchased from Wuyi Huacheng (Lianyungang) Plastic Technology Co., Ltd., brand CB7093H.

[0063] Examples 1 to 6 and Comparative Examples 1 to 6

[0064] Examples 1 to 6 and Comparative Examples 1 to 6 respectively provide a PC composite material, and the components and amounts thereof are shown in Table 1 and Table 2;

[0065] In Tables 1 and 2, the dosage units of each component are "parts by weight";

[0066] Table 1

[0067]

[0068] Table 2

[0069]

[0070] The preparation methods of the PC composite materials provided in Examples 1 to 6 and Comparative Examples 1 to 6 include the following steps:

[0071] (1) drying PCR-PC, carbon fiber (glass fiber and / or conductive carbon black), toughening agent, chain extender, lubricant, PC resin, antioxidant and masterbatch at 85° C. for 2 h to obtain a dry material;

[0072] (2) stirring all the dry materials except the dry carbon fiber (dried glass fiber) in a high-speed mixer for 10 min at a stirring speed of 600 rpm to obtain a mixed material;

[0073] (3) adding the mixed material into a twin-screw extruder, and adding dry carbon fiber from a side feed port, and obtaining the PC composite material through extrusion, cooling, granulation and drying;

[0074] Among them, the 11 temperature zones of the twin-screw extruder are set to 170°C, 255°C, 255°C, 250°C, 250°C, 245°C, 245°C, 240°C, 240°C, 250°C and 250°C respectively. The feeding speed of the twin-screw extruder is 15rpm and the main engine speed is 350rpm.

[0075] Performance Testing:

[0076] (1) Tensile strength: The PC composite material was injection molded to obtain test specimens, which were then tested according to the method provided in GB / T1040;

[0077] (2) Flexural strength: The PC composite material was injection molded to obtain test specimens, which were then tested according to the method provided in GB / T9341;

[0078] (3) Notched impact strength: The PC composite material was injection molded to obtain test specimens, which were then tested according to the method provided in GB / T1843;

[0079] (4) Surface resistivity at room temperature and after 7 days in a water bath at 70°C: The PC composite material was injection molded to obtain test specimens, which were then tested according to the method provided in GB / T 1410.

[0080] The PC composite materials provided in Examples 1 to 6 and Comparative Examples 1 to 6 were tested according to the above test method. The test results are shown in Table 3:

[0081] Table 3

[0082]

[0083]

[0084] According to the data in Table 3, we can see that:

[0085] The PC composite materials provided in Examples 1 to 6 have a tensile strength of 95 to 132 MPa, a flexural strength of 127 to 183 MPa, and a notched impact strength of 8.6 to 18.2 kJ / m 2 , the surface resistivity at room temperature is 10 7 ~10 10 Ω / m 2 , the surface resistivity after 7 days in a water bath at 70°C is 10 7 ~10 10 Ω / m 2 , with excellent antistatic performance, impact resistance, tensile performance and water and heat aging resistance;

[0086] Among them, by further optimizing the toughening agent, the PC composite materials provided in Examples 1 to 4 can have a tensile strength of up to 107 to 132 MPa, a flexural strength of up to 147 to 183 MPa, and a notched impact strength of up to 12.9 to 18.2 kJ / m 2 , the surface resistivity at room temperature is 10 7 ~10 10 Ω / m 2 , the surface resistivity after 7 days in a water bath at 70°C is 10 7 ~10 10 Ω / m 2 , with the best antistatic properties, impact resistance, tensile properties and water and heat aging resistance.

[0087] By comparing the data of Example 1 and Comparative Examples 1 to 3, it can be seen that the use of conductive carbon black and / or chopped glass fibers instead of chopped carbon fibers will lead to a decrease in the tensile strength and flexural strength of the resulting PC composite material, and an increase in the surface resistivity, indicating that the PC composite materials provided by Comparative Examples 1 to 3 have poor tensile properties and antistatic properties.

[0088] Comparing the data of Example 1 and Comparative Example 4, it can be seen that the chain extender is also very important. Failure to add the chain extender will lead to a decrease in the impact resistance and hydrothermal aging resistance of the obtained PC composite material.

[0089] Finally, by comparing the data of Example 1 and Comparative Examples 5 to 6, it can be seen that the amount of chopped carbon fiber added should not be too high or too low. If the amount of chopped carbon fiber added is too low, the surface resistivity of the resulting PC composite material will increase and the antistatic property will decrease. If the amount of chopped carbon fiber added is too high, the notched impact strength of the resulting PC composite material will decrease and the impact resistance will deteriorate.

[0090] The applicant declares that the present invention illustrates a PC composite material and its preparation method and application through the above embodiments, but the present invention is not limited to the above embodiments, that is, it does not mean that the present invention must rely on the above embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A PC composite material, It is characterized in that The PC composite material comprises the following components in parts by weight:

2. The PC composite material according to claim 1, It is characterized in that The melting index of the PCR-PC is 20 to 35 g / 10 min.

3. The PC composite material according to claim 1 or 2, It is characterized in that The carbon fiber is chopped carbon fiber; Preferably, the length of the chopped carbon fibers is 4 to 8 mm.

4. The PC composite material according to any one of claims 1 to 3, It is characterized in that The toughening agent includes any one of acrylonitrile-butadiene-styrene copolymer, methyl methacrylate-butadiene-styrene terpolymer, methyl methacrylate-acrylate-silicone terpolymer or maleic anhydride grafted polyolefin elastomer or a combination of at least two thereof, preferably a combination of methyl methacrylate-acrylate-silicone terpolymer and maleic anhydride grafted polyolefin elastomer.

5. The PC composite material according to any one of claims 1 to 4, It is characterized in that The chain extender includes a styrene-glycidyl methacrylate copolymer.

6. The PC composite material according to any one of claims 1 to 5, It is characterized in that The lubricant includes pentaerythritol stearate and / or ethylene bis stearamide.

7. The PC composite material according to any one of claims 1 to 6, It is characterized in that The PC composite material further comprises any one or a combination of at least two of PC resin, antioxidant or masterbatch; Preferably, the content of PC resin in the PC composite material is ≤30 parts by weight; Preferably, the melt index of the PC resin is 8 to 17 g / 10 min; Preferably, the content of the antioxidant in the PC composite material is 0.1 to 0.5 parts by weight; Preferably, the antioxidant comprises a hindered phenol antioxidant and / or a phosphite antioxidant, and more preferably a combination of a hindered phenol antioxidant and a phosphite antioxidant; Preferably, the content of masterbatch in the PC composite material is 0.5 to 1.5 parts by weight; Preferably, the masterbatch comprises a black masterbatch; Preferably, the black masterbatch comprises a PC carrier and carbon black.

8. A method for preparing the PC composite material according to any one of claims 1 to 7, It is characterized in that The preparation method comprises: mixing PCR-PC, carbon fiber, toughening agent, chain extender, lubricant, optional PC resin, optional antioxidant and optional masterbatch, and obtaining the PC composite material through extrusion, cooling, granulation and drying.

9. The preparation method according to claim 8, It is characterized in that The preparation method comprises the following steps: (1) drying PCR-PC, carbon fiber, toughening agent, chain extender, lubricant, optionally PC resin, optionally antioxidant and optionally masterbatch to obtain a dry material; (2) mixing all dry materials except the dry carbon fiber to obtain a mixed material; (3) adding the mixed material into a twin-screw extruder, and adding dry carbon fiber from a side feed port, and obtaining the PC composite material through extrusion, cooling, granulation and drying; Preferably, the drying temperature in step (1) is 80-100° C.; Preferably, the drying time in step (1) is 1 to 2 hours; Preferably, the mixing time in step (2) is 6 to 10 minutes; Preferably, the mixing in step (2) is performed at a rotation speed of 600 to 800 rpm; Preferably, the operating temperature of the twin-screw extruder in step (3) is 180-255° C. Preferably, the feeding speed of the twin-screw extruder in step (3) is 12 to 24 rpm; Preferably, the main engine speed of the twin-screw extruder in step (3) is 220 to 600 rpm.

10. Use of the PC composite material according to any one of claims 1 to 7 in electronic and electrical components.

Citation Information

Patent Citations